Pyrite inhibitor and flotation method for silver-copper-zinc polymetallic ore

By using pyrite inhibitor adsorbents to reduce the floating ability of pyrite in silver-copper-zinc polymetallic minerals, the separation problem of pyrite and sphingoite is solved, the amount of lime is reduced, and the metal recovery rate is improved. The calcium ion content in the return water is reduced and the process conditions are improved.

CN119056586APending Publication Date: 2024-12-03CHINA UNIV OF MINING & TECH (BEIJING) +3
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410588619.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-13
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

During the mixing process of silver-copper-zinc polymetallic sulfide ore, it is difficult to effectively separate pyrite and sphingoite, and the use of a large amount of lime leads to scale and safety hazards in the return water pipeline, affecting the subsequent sorting process.

Method used

Using a pyrite inhibitor, including methimazole, alizarin red and ortho-carboxythiophenol, reduces the floating ability of pyrite by strong adsorption with copper and iron ions on the pyrite surface, and Reduce the amount of lime during zinc-sulfur separation and improve metal recovery.

Benefits of technology

It effectively reduces the floating ability of pyrite, improves metal recovery, reduces the calcium ion content in the ore dressing return water, reduces the amount of lime, and improves subsequent process conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of mineral separation, in particular to a flotation method for a pyrite inhibitor and silver-copper-zinc polymetallic ore. The pyrite inhibitor provided by the invention is prepared from the following components in parts by mass: 1 to 2 parts of methimazole, 0.5 to 1.5 parts of alizarin red and 0.5 to 1.5 parts of o-carboxythiophenol. According to the flotation method of the silver-copper-zinc polymetallic ore, the pyrite inhibitor is adopted. The pyrite inhibitor can greatly reduce the floatability of pyrite and improve the metal recovery rate, and can be used for replacing lime; when the flotation agent is used for flotation of silver-copper-zinc polymetallic ore, the grade and the recovery rate of silver, copper and zinc can be improved on the basis of greatly reducing the use amount of lime.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ore dressing, in particular to a flotation method of pyrite inhibitor and silver-copper-zinc polymetallic ore. Background Art

[0002] In the flotation process of low-grade polymetallic ores, sulfide ore mixed flotation is a common process. The mixed flotation process is to first obtain mixed flotation concentrate by adding a large amount of activators and collectors, and then, according to the differences in the properties of each mineral, change the pH of the flotation slurry or add flotation inhibitors to achieve the selective separation of the target minerals in the mixed flotation concentrate.

[0003] In the mixed flotation process of silver, copper and zinc polymetallic sulfide ores, a large amount of copper sulfate is often added as an activator to improve the floatability of sphalerite and pyrite. Since the floatability of pyrite and sphalerite after copper sulfate activation is similar, it is difficult to separate them effectively. Usually, a large amount of lime needs to be added as a pyrite inhibitor when separating zinc-sulfur mixed flotation concentrates, even up to 100kg / t. Although the use of a large amount of lime can promote the separation of zinc and sulfur, a large amount of calcium ions enter the mineral processing return water, resulting in serious scaling and blockage of the return water pipeline, and seriously affecting the subsequent separation process. In addition, pyrite suppressed by a large amount of lime needs to be activated and flotated with a large amount of sulfuric acid. However, sulfuric acid is extremely corrosive and easily produces a large amount of hydrogen sulfide and sulfur dioxide gas, which poses a huge safety hazard. Therefore, finding a new agent to reduce the amount of lime used in the separation of zinc and sulfur after mixed flotation is of great significance to the subsequent process in order to achieve zinc-sulfur separation efficiency and reduce the calcium ion content in mineral processing return water.

[0004] In view of this, this invention is proposed. Summary of the invention

[0005] The first object of the present invention is to provide a pyrite inhibitor which can significantly reduce the floatability of pyrite, improve metal recovery rate and can be used to replace lime.

[0006] The second object of the present invention is to provide a flotation method for silver-copper-zinc polymetallic ore, which improves the grade and recovery rate of silver, copper and zinc on the basis of significantly reducing the amount of lime used.

[0007] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted: The present invention provides a pyrite inhibitor, which comprises the following components in parts by mass: 1-2 parts of methimazole, 0.5-1.5 parts of alizarin red and 0.5-1.5 parts of o-carboxybenzenethiol.

[0008] The present invention also provides a flotation method for silver-copper-zinc polymetallic ore, which adopts the pyrite inhibitor as described above.

[0009] Furthermore, the flotation method of the silver-copper-zinc polymetallic ore comprises the following steps: S1, grinding and slurrying the raw ore to obtain slurry; S2, subjecting the ore pulp to silver-copper mixed flotation to obtain silver-copper mixed flotation concentrate and silver-copper mixed flotation tailings; S3, subjecting the silver-copper mixed flotation tailings to zinc-sulfur mixed flotation to obtain zinc-sulfur mixed flotation concentrate and zinc-sulfur mixed flotation tailings; S4, mixing the zinc-sulfur mixed flotation concentrate and the pyrite inhibitor and performing zinc-sulfur separation to obtain zinc concentrate.

[0010] Furthermore, in step S1, the average silver grade in the raw ore is 100-125 g / t, the average copper grade is 0.3%-0.4%, and the average zinc grade is 0.45%-0.52%.

[0011] Further, in step S2, the silver-copper mixed flotation includes: adding lime to the slurry to adjust the pH of the slurry to 10-11, adding a depressant, a collector and a frother for a rough selection, adding a collector for three scavenging selections, and adding a depressant for a secondary selection to obtain the silver-copper mixed flotation concentrate and the silver-copper mixed flotation tailings.

[0012] Furthermore, step S2 includes at least one of the following features (1) to (6); (1) The inhibitor includes at least one of DL-2-amino-3-mercaptopropionic acid, diethylenetriamine and triethanolamine; (2) The amount of the inhibitor added is 100-2800 g / t; (3) The collector includes at least one of tert-butyl xanthate propylene ester, ethionamide and butyl ammonium black medicine; (4) The amount of the collector added is 100-500 g / t; (5) The foaming agent includes tripropylene glycol methyl ether and / or pine oil; (6) The amount of the foaming agent added is 50-100 g / t.

[0013] Furthermore, in step S3, the zinc-sulfur mixed flotation includes: slurrying the silver-copper mixed flotation tailings, adjusting the pH to 6-7, adding an activator and a collector for a primary roughing, and then performing secondary cleaning and tertiary scavenging to obtain the zinc-sulfur mixed flotation concentrate and the zinc-sulfur mixed flotation tailings.

[0014] Furthermore, step S3 includes at least one of the following features (1) to (4); (1) The activator includes copper sulfate; (2) The amount of the activator added is 100-150 g / t; (3) The collector includes butyl xanthate; (4) The amount of the collector added is 50~500g / t.

[0015] Furthermore, in step S4, the zinc-sulfur separation comprises: adding lime to the slurry containing the zinc-sulfur mixed flotation concentrate to adjust the pH of the slurry to 11-12, adding a collector and the pyrite inhibitor for a roughing process, adding the pyrite inhibitor for a third cleaning process, and adding a collector for a second scavenging process to obtain the zinc concentrate.

[0016] Further, in step S4, the collector includes at least one of butyl xanthate propylene ester, ethylthiocarbamate, butyl ammonium black medicine and ethylthiocarbamate; And / or, the added amount of the collector is 50~2000g / t.

[0017] Compared with the prior art, the present invention has the following beneficial effects: 1. The pyrite inhibitor provided by the present invention can strongly adsorb the copper ions and iron ions on the surface of pyrite to form a strong hydrophilic substance, which greatly reduces the floatability of pyrite and improves the metal recovery rate, and can be used to replace lime.

[0018] 2. The flotation method of silver, copper and zinc polymetallic ore provided by the present invention adopts the above-mentioned pyrite inhibitor, which can reduce the amount of lime used in zinc-sulfur separation, improve the zinc-sulfur separation efficiency, reduce the calcium ion content in the ore dressing return water, and reduce the impact of calcium ions on subsequent processes; and is beneficial to improving the grade and recovery rate of silver, copper and zinc. DETAILED DESCRIPTION

[0019] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but it will be appreciated by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work, all belong to the scope of protection of the present invention. If specific conditions are not indicated in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0020] In some embodiments of the present invention, a pyrite inhibitor is provided, which comprises the following components in parts by mass: 1-2 parts of methimazole, 0.5-1.5 parts of alizarin red and 0.5-1.5 parts of o-carboxybenzenethiol.

[0021] The present invention adopts a pyrite inhibitor prepared with methimazole, alizarin red and o-carboxylbenzenethiol. The -NH2 and -SO3 groups in the molecule can strongly adsorb copper ions and iron ions on the surface of pyrite to form a strong hydrophilic substance, which greatly reduces the floatability of pyrite and improves metal recovery. The pyrite inhibitor can be used to replace lime.

[0022] The pyrite inhibitor of the present invention contains -NH2 groups and -SO3 groups; wherein, the -NH2 groups can be complexed with copper ions or lead ions, thereby reducing the adsorption of the collector on the surface of pyrite; and the -SO3 groups are complexed with iron ions on the surface of pyrite to form an oxide film on the surface of pyrite, thereby reducing the floatability of pyrite. On the other hand, since the oxidizability of the Fe-S bond on the surface of pyrite is weaker than that of chalcopyrite and sphalerite, at this time, the adsorption of the -SO3 groups on the surface of pyrite is stronger than that of chalcopyrite and sphalerite. Due to this difference, there are differences in the collectability of chalcopyrite, sphalerite and pyrite, thereby achieving efficient separation of chalcopyrite, sphalerite and pyrite.

[0023] In some embodiments of the present invention, the pyrite inhibitor comprises the following components in parts by mass: 1-2 parts of methimazole, 0.8-1.2 parts of alizarin red and 0.8-1.2 parts of o-carboxybenzenethiol.

[0024] In some embodiments of the present invention, the pyrite depressant is a pyrite depressant for flotation of silver-copper-zinc polymetallic ores.

[0025] In some embodiments of the present invention, a method for preparing the above-mentioned pyrite inhibitor is also provided, comprising the following steps: After the components are mixed, a pyrite inhibitor is obtained.

[0026] In some embodiments of the present invention, a flotation method for silver-copper-zinc polymetallic ore is also provided, using the above-mentioned pyrite inhibitor.

[0027] The pyrite inhibitor of the present invention is used in the flotation of silver-copper-zinc polymetallic ores, and can recover silver, copper and zinc in the minerals with high yields on the basis of greatly reducing the amount of lime used, which is beneficial to improving the grade and recovery rate of silver, copper and zinc.

[0028] It should also be noted that the pyrite inhibitor that inhibits sulfur adsorption on the pyrite surface forms a feedback π bond with the mineral surface. At this time, the collector adsorbs on the pyrite surface to form a weaker δ bond, which reduces the adsorption of the collector on the pyrite surface.

[0029] In some embodiments of the present invention, the flotation method of silver-copper-zinc polymetallic ore comprises the following steps: S1, grinding and slurrying the raw ore to obtain slurry; S2, subjecting the ore pulp to silver-copper mixed flotation to obtain silver-copper mixed flotation concentrate and silver-copper mixed flotation tailings; S3, subjecting the silver-copper mixed flotation tailings to zinc-sulfur mixed flotation to obtain zinc-sulfur mixed flotation concentrate and zinc-sulfur mixed flotation tailings; S4. Mix the zinc-sulfur mixed flotation concentrate and the pyrite depressant and separate the zinc and sulfur to obtain zinc concentrate.

[0030] In some embodiments of the present invention, in step S1, the average silver grade in the original ore is 100-125 g / t, the average copper grade is 0.3%-0.4%, and the average zinc grade is 0.45%-0.52%; preferably, the average sulfur grade in the original ore is 6.5%-7.5%.

[0031] In some embodiments of the present invention, in step S1, the raw ore is a silver-copper-zinc polymetallic ore, wherein the metal minerals in the raw ore include at least one of silver, chalcopyrite, sphalerite, pyrite, galena and cassiterite, and the gangue minerals include at least one of quartz, fluorite, muscovite and calcite.

[0032] In some embodiments of the present invention, in step S1, the raw ore is ground so that the mass of solid particles with a particle size of ≤0.25 mm accounts for 70% to 85% of the total mass of the solid particles to obtain a grinding material.

[0033] In some embodiments of the present invention, in step S1, water is added to the grinding material for slurry adjustment to obtain slurry, and the mass concentration of the slurry is 25% to 40%.

[0034] In some embodiments of the present invention, in step S2, the silver-copper mixed flotation includes: adding lime to the slurry to adjust the pH of the slurry to 10-11, adding an inhibitor, a collector and a frother for a rough selection, adding a collector for three scavenging selections, and adding an inhibitor for a secondary selection to obtain a silver-copper mixed flotation concentrate and a silver-copper mixed flotation tailings.

[0035] In some embodiments of the present invention, in step S2, the inhibitor includes at least one of DL-2-amino-3-mercaptopropionic acid, diethylenetriamine and triethanolamine; preferably, in step S2, the inhibitor includes DL-2-amino-3-mercaptopropionic acid, diethylenetriamine and triethanolamine in a mass ratio of (1~2): (0.5~1.5): (1~2).

[0036] In some embodiments of the present invention, in step S2, the amount of inhibitor added is 100-2800 g / t.

[0037] In some embodiments of the present invention, in step S2, the collector includes at least one of tert-butyl xanthate propylene glycol, ethionamide and butyl ammonium black medicine; preferably, in step S2, the collector includes tert-butyl xanthate propylene glycol, ethionamide and butyl ammonium black medicine in a mass ratio of 1: (1~2): (0~2); more preferably, in step S2, the collector includes tert-butyl xanthate propylene glycol, ethionamide and butyl ammonium black medicine in a mass ratio of 1: (1~2): (1~2).

[0038] In some embodiments of the present invention, in step S2, the amount of collector added is 100-500 g / t.

[0039] In some embodiments of the present invention, in step S2, the foaming agent includes tripropylene glycol methyl ether and / or pine oil; preferably, in step S2, the foaming agent includes tripropylene glycol methyl ether and pine oil in a mass ratio of (0.8~1.2):(0.8~1.2).

[0040] In some embodiments of the present invention, in step S2, the amount of foaming agent added is 50-100 g / t.

[0041] In some embodiments of the present invention, in step S2, silver-copper mixed flotation specifically comprises the following steps: After adding lime to the pulp to adjust the pH value of the pulp to 10-11, 1500-2800 g / t of depressant, 300-500 g / t of collector and 50-100 g / t of frother are added to perform a roughing operation to obtain a roughing concentrate and a roughing tailing. Add 100-400g / t collector to the roughing tailings for the first scavenging to obtain scavenging tailings I and scavenging middling I; scavenging middling I is subjected to the second scavenging to obtain scavenging tailings II and scavenging middling II; scavenging middling II is subjected to the third scavenging to obtain scavenging tailings III (silver-copper mixed flotation tailings) and scavenging middling III; scavenging middling III is returned to the upper level operation; 500-1000 g / t of depressant is added to the rougher concentrate for the first concentration to obtain concentrated middlings IV and concentrated concentrate I. 100-300 g / t of depressant is added to the concentrated concentrate I for the second concentration to obtain silver-copper flotation concentrate and concentrated middlings V, and the concentrated middlings V are returned to the upper operation.

[0042] In some embodiments of the present invention, in step S3, zinc-sulfur mixed flotation includes: slurrying the silver-copper mixed flotation tailings, adjusting the pH to 6-7, adding an activator and a collector to perform a roughing selection, and then performing a secondary selection and a tertiary scavenging selection to obtain a zinc-sulfur mixed flotation concentrate and a zinc-sulfur mixed flotation tailings.

[0043] In some embodiments of the present invention, in step S3, the activator includes but is not limited to copper sulfate.

[0044] In some embodiments of the present invention, in step S3, the amount of activator added is 100-150 g / t.

[0045] In some embodiments of the present invention, in step S3, the collector includes but is not limited to butyl xanthate.

[0046] In some embodiments of the present invention, in step S3, the amount of collector added is 50-500 g / t.

[0047] In some embodiments of the present invention, in step S3, zinc-sulfur mixed flotation specifically comprises the following steps: Add water to the silver-copper mixed flotation tailings to adjust the slurry until the mass concentration of the slurry containing the silver-copper mixed flotation tailings is 35% to 40%; then add hydrochloric acid to adjust the pH of the system to 6 to 7; Adding 100-150 g / t of activator and 100-250 g / t of collector to the pH-adjusted silver-copper mixed flotation tailings slurry to perform a roughing operation to obtain roughing tailings and roughing concentrate; Add 200-500 g / t of collector to the rougher concentrate for the first concentration to obtain concentrated concentrate I and concentrated middlings I; add 300-500 g / t of collector to the concentrated concentrate I for the second concentration to obtain zinc-sulfur flotation concentrate and concentrated middlings II, and the concentrated middlings II are returned to the upper level operation; Add 50-250 g / t of collector to the rougher tailings for the first scavenging to obtain scavenged tailings III and scavenged tailings I; add 50-150 g / t of collector to the scavenged tailings I for the second scavenging to obtain scavenged tailings IV and scavenged tailings II; and perform the third scavenging on the scavenged tailings II to obtain zinc-sulfur flotation tailings and scavenged tailings V.

[0048] In some embodiments of the present invention, in step S4, zinc-sulfur separation includes: adding lime to the slurry containing zinc-sulfur mixed flotation concentrate to adjust the pH of the slurry to 11-12, adding a collector and a pyrite inhibitor for a roughing process, adding a pyrite inhibitor for a third cleaning process, and adding a collector for a second scavenging process to obtain a zinc concentrate.

[0049] In some embodiments of the present invention, in step S4, the collector includes at least one of butyl xanthate propylene ester, ethylthiocarbamate, butyl ammonium black medicine and ethylthiocarbamate.

[0050] In some embodiments of the present invention, in step S4, the amount of collector added is 50-2000 g / t.

[0051] In some embodiments of the present invention, in step S4, the amount of pyrite inhibitor added is 100-1000 g / t.

[0052] In some embodiments of the present invention, in step S4, zinc-sulfur separation comprises the following steps: After adding lime to the slurry containing zinc-sulfur mixed flotation concentrate to adjust the pH value of the slurry to 11-12, 1000-2000 g / t of collector and 500-1000 g / t of pyrite inhibitor are added to perform a roughing operation to obtain a roughing concentrate and a roughing tailing; Add 200-300 g / t of pyrite inhibitor to the rougher concentrate for the first concentration to obtain concentrated concentrate I and concentrated middlings I; add 100-200 g / t of pyrite inhibitor to the concentrated concentrate I for the second concentration to obtain concentrated concentrate II and concentrated middlings II; and perform the third concentration on the concentrated concentrate II to obtain zinc concentrate and concentrated middlings III; 200-300 g / t of collector is added to the rougher tailings for the first scavenging to obtain scavenged tailings IV and scavenged tailings I; 50-150 g / t of collector is added to the scavenged tailings I for the second scavenging to obtain scavenged tailings and scavenged tailings V.

[0053] In some embodiments of the present invention, the amount of each reagent added is the mass of the reagent added per ton of slurry.

[0054] In some embodiments of the present invention, the silver recovery rate of the flotation method of the silver-copper-zinc polymetallic ore is 90% to 95%, the copper recovery rate is 89% to 97%, and the zinc recovery rate is 90% to 96%.

[0055] Example 1 The flotation method of the silver-copper-zinc polymetallic ore provided in this embodiment comprises the following steps: S1. Grind the raw ore to make the particle size of -0.25mm account for 70.45%, and then add water to adjust the mass concentration of the slurry to 30.71%; The original ore is a silver-copper-zinc polymetallic ore; among them, metal minerals include silver, chalcopyrite, sphalerite and pyrite, and gangue minerals include quartz and muscovite; the average grades of silver, copper, zinc and sulfur in the original ore are 120g / t, 0.40%, 0.52% and 6.50% respectively.

[0056] S2, adding lime to the above pulp to adjust the pH of the pulp to 10; then adding 2800g / t of depressant, 500g / t of collector and 100g / t of frother to carry out a roughing, to obtain a roughing concentrate and a roughing tailing; 400g / t collector is added to the roughing tailings for the first scavenging to obtain scavenging tailings I and scavenging middling I; scavenging middling I is subjected to the second scavenging to obtain scavenging tailings II and scavenging middling II; scavenging middling II is subjected to the third scavenging to obtain scavenging tailings III (silver-copper mixed flotation tailings) and scavenging middling III; scavenging middling III is returned to the upper level operation; 1000 g / t of depressant is added to the rougher concentrate for the first concentration to obtain concentrated middlings IV and concentrated concentrates I; 100 g / t of depressant is added to the concentrated concentrate I for the second concentration to obtain silver-copper flotation concentrate and concentrated middlings V, and the concentrated middlings V are returned to the upper operation; The inhibitor is DL-2-amino-3-mercaptopropionic acid, diethylenetriamine and triethanolamine in a mass ratio of 1:1:1; the inhibitor is added in the form of an aqueous solution with a concentration of 2wt% of the inhibitor; The collector is tert-butyl xanthate propylene ester and ethylthiocarbamate in a mass ratio of 1:1; the collector is added in the form of an aqueous solution with a concentration of 2wt% of the collector; The foaming agent is pine oil.

[0057] S3, adding water to the silver-copper mixed flotation tailings to adjust the slurry until the mass concentration of the slurry containing the silver-copper mixed flotation tailings is 35%; then adding hydrochloric acid to adjust the pH of the system to 6; Adding 150 g / t of copper sulfate activator and 250 g / t of collector to the pH-adjusted silver-copper mixed flotation tailings slurry to perform a roughing operation to obtain roughing tailings and roughing concentrate; 200g / t of collector is added to the rougher concentrate for the first concentration to obtain concentrated concentrate I and concentrated middlings I; 300g / t of collector is added to the concentrated concentrate I for the second concentration to obtain zinc-sulfur flotation concentrate and concentrated middlings II; the concentrated middlings II are returned to the upper level operation; Add 50g / t of collector to the roughing tailings for the first scavenging to obtain scavenged tailings III and scavenged tailings I; add 50g / t of collector to the scavenged tailings I for the second scavenging to obtain scavenged tailings IV and scavenged tailings II; perform the third scavenging on scavenged tailings II to obtain zinc-sulfur flotation tailings and scavenged tailings V; scavenged tailings V are returned to the upper level operation; The collector is butyl xanthate.

[0058] S4, adding 2kg / t lime to the slurry containing zinc-sulfur mixed flotation concentrate to adjust the pH of the slurry to 11, and then adding 1000g / t collector and 500g / t pyrite inhibitor to perform a roughing, to obtain a roughing concentrate and a roughing tailing; 200 g / t pyrite inhibitor is added to the rougher concentrate for the first concentration to obtain concentrated concentrate I and concentrated middlings I; 100 g / t pyrite inhibitor is added to the concentrated concentrate I for the second concentration to obtain concentrated concentrate II and concentrated middlings II; the concentrated concentrate II is subjected to the third concentration to obtain zinc concentrate and concentrated middlings III; the concentrated middlings III are returned to the upper level operation; Add 200g / t of collector to the rougher tailings for the first scavenging to obtain scavenged tailings IV and scavenged tailings I; add 100g / t of collector to the scavenged tailings I for the second scavenging to obtain scavenged tailings and scavenged tailings V; scavenged tailings V are returned to the upper level operation; The pyrite inhibitor is methimazole, alizarin red and o-carboxythiophenol in a mass ratio of 1:1:1; The collector is ethionamide.

[0059] Example 2 The flotation method of the silver-copper-zinc polymetallic ore provided in this embodiment comprises the following steps: S1. Grind the raw ore to make the particle size of -0.25mm account for 80.65%, and then add water to adjust the mass concentration of the slurry to 34.33%; The original ore is a silver-copper-zinc polymetallic ore; among them, metal minerals include silver, chalcopyrite, sphalerite, pyrite and cassiterite, and gangue minerals include quartz and calcite; the average grades of silver, copper, zinc and sulfur in the original ore are 100g / t, 0.35%, 0.50% and 7.23% respectively.

[0060] S2, adding lime to the above pulp to adjust the pH of the pulp to 11; then adding 1500g / t of inhibitor, 300g / t of collector and 50g / t of frother to carry out a roughing, to obtain a roughing concentrate and a roughing tailing; 100g / t collector is added to the roughing tailings for the first scavenging to obtain scavenging tailings I and scavenging middling I; scavenging middling I is subjected to the second scavenging to obtain scavenging tailings II and scavenging middling II; scavenging middling II is subjected to the third scavenging to obtain scavenging tailings III (silver-copper mixed flotation tailings) and scavenging middling III; scavenging middling III is returned to the upper level operation; 500 g / t of depressant is added to the rougher concentrate for the first concentration to obtain concentrated middlings IV and concentrated concentrates I. 300 g / t of depressant is added to the concentrated concentrate I for the second concentration to obtain silver-copper flotation concentrate and concentrated middlings V, and the concentrated middlings V are returned to the upper operation. The inhibitor is DL-2-amino-3-mercaptopropionic acid, diethylenetriamine and triethanolamine in a mass ratio of 1:1:2; the inhibitor is added in the form of an aqueous solution with a concentration of 2wt% of the inhibitor; The collector is tert-butyl xanthate propylene ester, ethylthiocarbamate and butyl ammonium black medicine in a mass ratio of 1:1:2; the collector is added in the form of an aqueous solution of the collector with a concentration of 2wt%; The foaming agent is tripropylene glycol methyl ether and pine oil in a mass ratio of 1:1.

[0061] S3, adding water to the silver-copper mixed flotation tailings to adjust the slurry until the mass concentration of the slurry containing the silver-copper mixed flotation tailings is 38%; then adding hydrochloric acid to adjust the pH of the system to 7; Adding 150 g / t of copper sulfate activator and 100 g / t of collector to the pH-adjusted silver-copper mixed flotation tailings slurry to perform a roughing operation to obtain roughing tailings and roughing concentrate; 300g / t of collector is added to the rougher concentrate for the first concentration to obtain concentrated concentrate I and concentrated middlings I; 400g / t of collector is added to the concentrated concentrate I for the second concentration to obtain zinc-sulfur flotation concentrate and concentrated middlings II; the concentrated middlings II are returned to the upper level operation; 100 g / t of collector is added to the roughing tailings for the first scavenging to obtain scavenged tailings III and scavenged tailings I; 100 g / t of collector is added to the scavenged tailings I for the second scavenging to obtain scavenged tailings IV and scavenged tailings II; the scavenged tailings II is subjected to the third scavenging to obtain zinc-sulfur flotation tailings and scavenged tailings V; the scavenged tailings V are returned to the upper level operation; The collector is butyl xanthate.

[0062] S4, adding 3.5kg / t lime to the slurry containing zinc-sulfur mixed flotation concentrate to adjust the pH of the slurry to 12, and then adding 1500g / t collector and 1000g / t pyrite inhibitor to perform a roughing, to obtain a roughing concentrate and a roughing tailing; 250 g / t pyrite inhibitor is added to the rougher concentrate for the first concentration to obtain concentrated concentrate I and concentrated middlings I; 150 g / t pyrite inhibitor is added to the concentrated concentrate I for the second concentration to obtain concentrated concentrate II and concentrated middlings II; the concentrated concentrate II is subjected to the third concentration to obtain zinc concentrate and concentrated middlings III; the concentrated middlings III are returned to the upper level operation; Add 250g / t of collector to the rougher tailings for the first scavenging to obtain scavenged tailings IV and scavenged tailings I; add 150g / t of collector to the scavenged tailings I for the second scavenging to obtain scavenged tailings and scavenged tailings V; scavenged tailings V are returned to the upper level operation; The pyrite inhibitor is methimazole, alizarin red and o-carboxythiophenol in a mass ratio of 1.5:1:1; The collector is butyl xanthate.

[0063] Example 3 The flotation method of the silver-copper-zinc polymetallic ore provided in this embodiment comprises the following steps: S1. Grind the raw ore to make the particle size -0.25mm account for 84.50%, and then add water to adjust the concentration of the slurry to 38.45%; The original ore is a silver-copper-zinc polymetallic ore; among them, metal minerals include silver, chalcopyrite, sphalerite, pyrite and galena, and gangue minerals include quartz, fluorite and calcite; the average grades of silver, copper, zinc and sulfur in the original ore are 125g / t, 0.30%, 0.45% and 7.15% respectively.

[0064] S2, adding lime to the above pulp to adjust the pH of the pulp to 11; then adding 2300g / t of inhibitor, 400g / t of collector and 60g / t of frother to carry out a roughing, to obtain a roughing concentrate and a roughing tailing; Add 250g / t collector to the roughing tailings for the first scavenging to obtain scavenging tailings I and scavenging middling I; scavenging middling I is subjected to the second scavenging to obtain scavenging tailings II and scavenging middling II; scavenging middling II is subjected to the third scavenging to obtain scavenging tailings III (silver-copper mixed flotation tailings) and scavenging middling III; scavenging middling III is returned to the upper level operation; 800 g / t of depressant is added to the rougher concentrate for the first concentration to obtain concentrated middlings IV and concentrated concentrates I. 200 g / t of depressant is added to the concentrated concentrate I for the second concentration to obtain silver-copper flotation concentrate and concentrated middlings V, and the concentrated middlings V are returned to the upper operation. The inhibitor is DL-2-amino-3-mercaptopropionic acid, diethylenetriamine and triethanolamine in a mass ratio of 2:1:1; the inhibitor is added in the form of an aqueous solution with a concentration of 2wt% of the inhibitor; The collector is tert-butyl xanthate propylene ester, ethylthiocarbamate and butyl ammonium black medicine in a mass ratio of 1:2:1; the collector is added in the form of an aqueous solution of the collector with a concentration of 2wt%; The foaming agent is tripropylene glycol methyl ether and pine oil in a mass ratio of 1:1.

[0065] S3, adding water to the silver-copper mixed flotation tailings to adjust the slurry until the mass concentration of the slurry containing the silver-copper mixed flotation tailings is 40%; then adding hydrochloric acid to adjust the pH of the system to 7; Adding 150 g / t of copper sulfate activator and 200 g / t of collector to the pH-adjusted silver-copper mixed flotation tailings slurry to perform a roughing operation to obtain roughing tailings and roughing concentrate; 450g / t of collector is added to the rougher concentrate for the first concentration to obtain concentrated concentrate I and concentrated middlings I; 400g / t of collector is added to the concentrated concentrate I for the second concentration to obtain zinc-sulfur flotation concentrate and concentrated middlings II; the concentrated middlings II are returned to the upper level operation; Add 200g / t of collector to the roughing tailings for the first scavenging to obtain scavenged tailings III and scavenged tailings I; add 100g / t of collector to the scavenged tailings I for the second scavenging to obtain scavenged tailings IV and scavenged tailings II; perform the third scavenging on scavenged tailings II to obtain zinc-sulfur flotation tailings and scavenged tailings V; scavenged tailings V are returned to the upper level operation; The collector is butyl xanthate.

[0066] S4, adding 3kg / t lime to the slurry containing zinc-sulfur mixed flotation concentrate to adjust the pH of the slurry to 12, and then adding 2000g / t collector and 1000g / t pyrite inhibitor to perform a roughing, to obtain a roughing concentrate and a roughing tailings; 300 g / t pyrite inhibitor is added to the rougher concentrate for the first concentration to obtain concentrated concentrate I and concentrated middlings I; 200 g / t pyrite inhibitor is added to the concentrated concentrate I for the second concentration to obtain concentrated concentrate II and concentrated middlings II; the concentrated concentrate II is subjected to the third concentration to obtain zinc concentrate and concentrated middlings III; the concentrated middlings III are returned to the upper level operation; 300 g / t of collector is added to the rougher tailings for the first scavenging to obtain scavenged tailings IV and scavenged tailings I; 100 g / t of collector is added to the scavenged tailings I for the second scavenging to obtain scavenged tailings and scavenged tailings V; scavenged tailings V are returned to the upper level operation; The pyrite inhibitor is methimazole, alizarin red and o-carboxybenzenethiol in a mass ratio of 2:1:1; The collector is butyl ammonium black medicine and ethionamide in a mass ratio of 1:2.

[0067] Example 4 The flotation method of silver-copper-zinc polymetallic ore provided in this embodiment refers to Example 3, except that, in step S4, the pyrite inhibitor is methimazole, alizarin red and o-carboxythiophenol in a mass ratio of 1:2:2.

[0068] Example 5 The flotation method for silver-copper-zinc polymetallic ore provided in this embodiment refers to Example 3, except that, in step S2, the inhibitor is DL-2-amino-3-mercaptopropionic acid, diethylenetriamine and triethanolamine in a mass ratio of 1:2:1.

[0069] Comparative Example 1 The flotation method of silver-copper-zinc polymetallic ore provided in this comparative example refers to Example 3, except that in step S4, the pyrite inhibitor is lime and sodium humate in a mass ratio of 3:1; the amount of lime in the pyrite inhibitor is 51 kg / t.

[0070] Test Example 1 The grades and yields of silver, copper and zinc obtained by the flotation method of the silver-copper-zinc polymetallic ore of Examples 1 to 5 and Comparative Example 1 are shown in Table 1.

[0071] Table 1

[0072] It can be seen from Table 1 that, compared with using lime as an inhibitor, the pyrite inhibitor of the present invention can significantly reduce the amount of lime used and improve the grade and recovery rate of silver, copper and zinc.

[0073] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A pyrite inhibitor, characterized in that: According to the mass percentage, it includes the following components: 1-2 parts of methimazole, 0.5-1.5 parts of alizarin red and 0.5-1.5 parts of o-carboxybenzenethiol.

2. A flotation method for silver-copper-zinc polymetallic ore, characterized in that: The pyrite inhibitor according to claim 1 is used.

3. The flotation method of silver-copper-zinc polymetallic ore according to claim 2, characterized in that: The steps include: S1, grinding and slurrying the raw ore to obtain slurry; S2, subjecting the ore pulp to silver-copper mixed flotation to obtain silver-copper mixed flotation concentrate and silver-copper mixed flotation tailings; S3, subjecting the silver-copper mixed flotation tailings to zinc-sulfur mixed flotation to obtain zinc-sulfur mixed flotation concentrate and zinc-sulfur mixed flotation tailings; S4, mixing the zinc-sulfur mixed flotation concentrate and the pyrite inhibitor and performing zinc-sulfur separation to obtain zinc concentrate.

4. The flotation method of silver-copper-zinc polymetallic ore according to claim 3, characterized in that: In step S1, the average silver grade in the raw ore is 100-125 g / t, the average copper grade is 0.3%-0.4%, and the average zinc grade is 0.45%-0.52%.

5. The flotation method of silver-copper-zinc polymetallic ore according to claim 3, characterized in that: In step S2, the silver-copper mixed flotation includes: adding lime to the slurry to adjust the pH of the slurry to 10-11, adding a depressant, a collector and a frother for a roughing selection, adding a collector for three scavenging selections, and adding a depressant for a secondary selection to obtain the silver-copper mixed flotation concentrate and the silver-copper mixed flotation tailings.

6. The flotation method of silver-copper-zinc polymetallic ore according to claim 5, characterized in that: In step S2, at least one of the following features (1) to (6) is included; (1) The inhibitor includes at least one of DL-2-amino-3-mercaptopropionic acid, diethylenetriamine and triethanolamine; (2) The amount of the inhibitor added is 100-2800 g / t; (3) The collector includes at least one of tert-butyl xanthate propylene ester, ethionamide and butyl ammonium black medicine; (4) The amount of the collector added is 100-500 g / t; (5) The foaming agent includes tripropylene glycol methyl ether and / or pine oil; (6) The amount of the foaming agent added is 50-100 g / t.

7. The flotation method of silver-copper-zinc polymetallic ore according to claim 3, characterized in that: In step S3, the zinc-sulfur mixed flotation includes: slurrying the silver-copper mixed flotation tailings, adjusting the pH to 6-7, adding an activator and a collector for a roughing selection, and then performing a secondary selection and a tertiary scavenging to obtain the zinc-sulfur mixed flotation concentrate and the zinc-sulfur mixed flotation tailings.

8. The flotation method of silver-copper-zinc polymetallic ore according to claim 7, characterized in that: In step S3, at least one of the following features (1) to (4) is included; (1) The activator includes copper sulfate; (2) The amount of the activator added is 100-150 g / t; (3) The collector includes butyl xanthate; (4) The amount of the collector added is 50~500g / t.

9. The flotation method of silver-copper-zinc polymetallic ore according to claim 3, characterized in that: In step S4, the zinc-sulfur separation includes: adding lime to the slurry containing the zinc-sulfur mixed flotation concentrate to adjust the pH of the slurry to 11-12, adding a collector and the pyrite inhibitor to perform a roughing selection, adding the pyrite inhibitor to perform a third concentration, and adding a collector to perform a second scavenging selection to obtain the zinc concentrate.

10. The flotation method of silver-copper-zinc polymetallic ore according to claim 9, characterized in that: In step S4, the collector includes at least one of butyl xanthate propylene ester, ethylthiocarbamate, butyl ammonium black medicine and ethylthiocarbamate; And / or, the added amount of the collector is 50~2000g / t.

Citation Information

Cited By

  • Flotation reagent for high-sulfur lead zinc ore in low-alkali environment

    CN119327624A

  • Beneficiation method for recovering silver, copper, zinc and sulfur from complex table middlings

    CN119972342A