Small-specification high-strength low-plasticity special wire preparation system and method

An integrated system and method for producing small-sized high-strength wires addresses cracking issues by directly forming molten steel into wire, reducing production time and increasing yield, thus overcoming conventional process limitations.

CN119057030AActive Publication Date: 2024-12-03HEBEI DAHE MATERIAL TECH CO LTD +2
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411114159.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-12-03
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

Conventional wire preparation processes for high-strength, low-plasticity materials are lengthy, complex, and prone to cracking, leading to low yield and high costs due to material loss and extended production times.

Method used

An integrated system and method utilizing a melting furnace, drainage pipe, cooling device, induction heating, and winder, with controlled argon pressure and nitrogen regulation, to produce small-sized high-strength wires by solidifying molten steel directly into wire form, avoiding traditional forging and rolling steps.

Benefits of technology

The method significantly reduces production time by over 80% and increases yield by more than 40%, producing high-strength wires with minimal deformation and material loss, while enabling production of various specifications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119057030A_ABST
    Figure CN119057030A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation system and method for a small-specification high-strength low-plasticity special wire. The preparation system comprises a smelting furnace, a drainage pipe, a cooling device, an induction heating device, a winder, a nitrogen pressure regulation and control device and an argon filling device. A gas inlet is formed in the top of the smelting furnace, and the argon filling device is communicated with the gas inlet through the nitrogen pressure regulation and control device; a discharge hole is formed in the bottom of the smelting furnace; one end of the drainage pipe is communicated with the discharge hole; the cooling device is used for cooling the drainage pipe and molten steel in the drainage pipe; the induction heating device is used for heating the wire output from the other end of the drainage tube; and the winder is used for winding the wire rod heated by the induction heating device. According to the system and method, steel ingot casting, blank forging, hot rolling, solid solution, drawing and other procedures are omitted, plastic deformation of materials can be avoided, the construction period is shortened by 80% or above, meanwhile, material loss in the forging, hot rolling and drawing processes is avoided, and the yield is increased by 40% or above; and products with different specifications can be prepared according to wire requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of metal material processing and forming, and in particular to a system and method for preparing small-sized high-strength and low-plasticity special wires. Background Art

[0002] At present, the demand for wire products is very large. The conventional wire preparation process is smelting + refining + forging (continuous casting) + rolling + drawing, and the process is long and complicated. Some high-alloy special materials have crack defects during the hot and cold deformation processes such as forging, rolling, and drawing due to their poor plasticity and high strength. Small-specification wire products cannot be prepared, which greatly affects the material yield and service capacity. In severe cases, the product may break and be scrapped. In order to meet product supply requirements, some manufacturers need to prepare wire from steel ingots through wire cutting, turning, etc., and the processing cost, time cost, and raw material cost are very expensive. This problem needs to be solved urgently. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a small-size high-strength low-plasticity special wire preparation system that realizes integrated preparation; the present invention also provides a small-size high-strength low-plasticity special wire preparation method.

[0004] In order to solve the above technical problems, the technical solution adopted by the present invention is: it includes a melting furnace, a drainage pipe, a cooling device, an induction heating device, a winder, a nitrogen pressure control device and an argon filling device; an air inlet is provided at the top of the melting furnace, and the argon filling device is connected to the air inlet through the nitrogen pressure control device; a discharge port is provided at the bottom of the melting furnace, and one end of the drainage pipe is connected to the discharge port; the cooling device is used to cool the drainage pipe and the molten steel inside it; the induction heating device is used to heat the wire output from the other end of the drainage pipe; and the winder is used to wind up the wire heated by the induction heating device.

[0005] Furthermore, the drainage tube has several models according to the wire specifications.

[0006] Furthermore, the cooling device includes a cooling pipe and a coolant circulation device; the cooling pipe is coiled outside the drainage pipe.

[0007] Furthermore, it also includes a guide wheel; the guide wheel is used to guide the wire heated by the induction heating device to the winder.

[0008] Furthermore, a pressure sensor is provided in the smelting furnace; the nitrogen pressure regulating device is provided with a flow control valve and a flow controller; the flow controller regulates the flow control valve through the pressure feedback from the pressure sensor.

[0009] In order to solve the above technical problems, the present invention adopts the above system, and the technical solution adopted includes the following steps: 1) according to the wire composition requirements, the alloy raw materials are put into the melting furnace, vacuuming, heating, and refining until the composition meets the wire product requirements;

[0010] 2) Filling argon into the melting furnace, and determining the argon pressure in the melting furnace according to the wire diameter and the finished product winding speed requirements; the argon pressure P in the melting furnace is calculated using the following formula (I);

[0011]

[0012] In formula (I), v is the winding rate, mm / min; d is the finished wire diameter, mm; P is the argon filling pressure, Pa; e is a natural constant;

[0013] 3) The molten steel in the smelting furnace flows into the drainage pipe under the pressure of argon gas, and is cooled by the cooling device to solidify into wire;

[0014] 4) The wire output from the drainage tube is heated by an induction heating device and then reeled on a reel.

[0015] Furthermore, the drainage tube is replaced with a corresponding model according to the wire specifications.

[0016] Furthermore, in step 4), the wire is heated by the induction heating device and then guided to the winder through a guide wheel.

[0017] The beneficial effects of adopting the above technical scheme are: the present invention can solve the forging and drawing cracking problems in the preparation process of high-strength, low-plasticity wire products, and prepare wire products in an integrated manner; the system and method of the present invention omits the processes of ingot casting, billet forging, hot rolling, solutionizing, drawing, etc., which can effectively avoid plastic deformation of materials and shorten the construction period by more than 80%, while avoiding material loss in the forging, hot rolling and drawing processes, and increasing the yield rate by more than 40%; different specifications of products can be prepared according to wire requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0019] Figure 1 It is a structural schematic diagram of the system of the present invention;

[0020] Figure 2 This is a photo of severe cracking of the steel ingot in Example 1 during forging;

[0021] Figure 3 This is a photo of severe cracking during wire rolling in Example 2.

[0022] In the figure: a smelting furnace 1, an adapter 2, a drainage pipe 3, a cooling device 4, an induction heating device 5, a guide wheel 6, a winder 7, a wire 8, a nitrogen pressure regulating device 9, an argon filling device 10, and an argon supply device 11. DETAILED DESCRIPTION

[0023] Figure 1 As shown, the small-size high-strength low-plasticity special wire preparation system includes a smelting furnace 1, a drainage pipe 3, a cooling device 4, an induction heating device 5, a guide wheel 6, a winder 7, a nitrogen pressure control device 9 and an argon filling device 10. The top of the smelting furnace 1 is provided with an air inlet and a pressure sensor, and the argon filling device 10 is connected to the air inlet of the smelting furnace 1 through the nitrogen pressure control device 9. The nitrogen pressure control device 9 is provided with a flow control valve and a flow controller; the flow controller controls the flow control valve through the pressure feedback from the pressure sensor. An argon supply device 11 is also provided to provide argon to the argon filling device 10.

[0024] Figure 1 As shown, in the small-size high-strength low-plasticity special wire preparation system, the bottom of the smelting furnace 1 is provided with a discharge port, and one end of the drainage pipe 3 is connected to the discharge port of the smelting furnace 1. The drainage pipe 3 has several models according to the wire specifications, and can be connected to the discharge port of the smelting furnace 1 through an adapter 2; the adapter 2 is provided with a valve. The cooling device 4 is used to cool the drainage pipe 3 and the molten steel inside it; the cooling device 4 is preferably: including a cooling pipe and a coolant circulation device, the cooling pipe is coiled on the outside of the drainage pipe 3, and the two ends of the cooling pipe are connected to the coolant circulation device; in this way, the coolant is powered by the coolant circulation device, and the coolant circulates in the cooling pipe coil, thereby realizing the cooling of the drainage pipe 3 and the molten steel inside it.

[0025] Figure 1 As shown, in the small-size high-strength low-plasticity special wire preparation system, the induction heating device 5 is used to heat the wire 8 output from the other end of the drainage tube 3; the induction heating device 5 preferably includes an induction power supply and an induction coil, and the wire 8 passes through the induction coil; in this way, the induction coil can heat the wire 8 passing through. The guide wheel 6 is used to guide and bend the wire 8 heated by the induction heating device 5 to the reel 7, and a number of guide wheels 6 are provided as needed. The reel 7 is used to reel the wire 8 heated by the induction heating device 5 and guided into by the guide wheel 6.

[0026] Figure 1 As shown, the method for preparing small-sized high-strength low-plasticity special wire comprises the following steps:

[0027] 1) Replace the drainage tube 3 with the corresponding model according to the wire specifications. Add the alloy raw materials into the smelting furnace 1 according to the wire composition requirements, evacuate to <1Pa, and heat to melt and refine the alloy raw materials until the composition meets the wire product requirements;

[0028] 2) Argon is charged into the melting furnace 1, and the argon pressure in the melting furnace 1 is determined according to the wire diameter and the finished product winding speed requirements; the argon pressure P in the melting furnace is calculated using the following formula (I);

[0029]

[0030] In formula (I), v is the winding rate, mm / min; d is the finished wire diameter, mm; P is the argon filling pressure, Pa; e is a natural constant;

[0031] 3) The molten steel in the smelting furnace 1 flows into the drainage pipe 3 under the pressure of argon gas, and is cooled by the cooling device 4 to solidify into the wire 8;

[0032] 4) The wire output from the drainage tube 3 is heated by the induction heating device 5 to soften the wire, and is then guided and bent by the guide wheel 6 and finally reeled on the reel 7.

[0033] This method is suitable for preparing wires with a specification of 6 to 10 mm, and the preparation speed of the finished wires is 1000 to 1500 mm / min.

[0034] Example 1: In this example, a 6.0 mm diameter high-strength Ni-Cr-W alloy is prepared. Since it has a serious tendency to crack during hot working, it cannot be prepared by hot working. Instead, it is prepared by the following method:

[0035] According to the required wire diameter of 6mm and the finished product winding speed requirement of 1000mm / min, replace the 6mm specification drainage tube 3. According to the alloy composition requirements, the raw materials required for smelting are added to the crucible of the smelting furnace 1 according to the content requirements, and the vacuum is evacuated to <1Pa, then the temperature is raised to melt and refine until the composition meets the wire product requirements. Open the flow control valve of the nitrogen pressure control device 9, and determine the pressure in the smelting furnace according to formula (I) The valve of the adapter 2 is opened, and the molten steel flows into the drainage pipe 3. The argon pressure in the furnace pushes the molten steel to flow slowly at a stable rate in the drainage pipe 3. After passing through the cooling device 4, the molten steel is slowly cooled and solidified to form a wire 8 of a certain specification. The wire continues to move forward, is heated by the induction heating device 5 to soften the wire, and continues to move to the guide wheel 6 to achieve wire coiling, and finally is coiled on the coiling system.

[0036] Example 2: This example prepares 8.0 mm diameter Ni55Cr40 alloy. Because of its severe tendency to crack during hot working and tight production cycle, conventional smelting-forging-rolling process cannot meet the supply requirements, and the preparation is carried out by the following method:

[0037] According to the required wire diameter of 8.0mm and the finished product winding speed requirement of 1300mm / min, replace the 8.0mm specification drainage tube 3. According to the alloy composition requirements, the raw materials required for smelting are added to the crucible of the smelting furnace 1 according to the content requirements, and the vacuum is evacuated to <1Pa, then the temperature is raised to melt and refine until the composition meets the wire product requirements. Open the flow control valve of the nitrogen pressure control device 9, and determine the pressure in the smelting furnace as P=0.81MPa according to formula (I). Open the valve of the adapter 2, and the molten steel flows into the drainage tube 3. Relying on the argon pressure in the furnace, the molten steel is pushed to flow slowly at a stable rate in the drainage tube 3. After passing through the cooling device 4, the molten steel is slowly cooled and solidified to form a wire 8 of a certain specification. The wire continues to move forward, and the wire is softened by heating by the induction heating device 5, and continues to move to the guide wheel 6 to achieve wire curling, and finally achieves winding on the winding system.

[0038] The finished wire rod obtained in this embodiment has a smooth surface and standard size.

[0039] Example 3: This example prepares a 10.0 mm diameter Ni58Cr16Mo16W4Fe5 nickel-based alloy, which has a serious tendency to deformation and work hardening and cannot be formed by forging. The preparation is carried out by the following method:

[0040] According to the required wire diameter of 10.0mm and the finished product winding speed requirement of 1500mm / min, replace the 10.0mm specification cooling tube. According to the alloy composition requirements, the raw materials required for smelting are added to the crucible of the smelting furnace 1 according to the content requirements, and the vacuum is evacuated to <1Pa, then the temperature is raised to melt and refine until the composition meets the wire product requirements. Open the flow control valve of the nitrogen pressure regulating device 9, and determine the pressure in the smelting furnace as P=1.08MPa according to formula (Ⅰ). Open the valve of the adapter 2, and the molten steel flows into the drainage pipe 3. Relying on the argon pressure in the furnace, the molten steel is pushed to flow slowly at a stable rate in the drainage pipe 3. After passing through the cooling device 4, the molten steel is slowly cooled and solidified to form a wire 8 of a determined specification. The wire continues to move forward, and the wire is softened by heating by the induction heating device 5, and continues to move to the guide wheel 6 to achieve wire curling, and finally achieves winding on the winding system.

[0041] The finished wire rod obtained in this embodiment has a smooth surface and standard size.

[0042] Comparative Example 1: Ni-Cr-W alloy wire with a diameter of 6 mm was prepared by smelting-forging-rolling process. When the steel ingot was forged, severe cracking occurred. Figure 2 , requiring multiple grindings and huge losses, with a yield rate of only 51%.

[0043] Comparative Example 2: Preparation of φ10mmNi58Cr16Mo16W4Fe5 nickel-based alloy wire products, poor hot working plasticity leads to severe rolling cracking, see Figure 3 , all products are scrapped. At the same time, the production cycle of this product is 20 working days, and the production pace is too slow.

[0044] The comparison of the yield rate and production cycle of Examples 1-3 and Comparative Examples 1-2 is shown in Table 1;

[0045] Table 1: Comparison of yield rate and production cycle

[0046]

[0047] As can be seen from Table 1, the system and method effectively improve the yield rate of wire rods and shorten the production cycle.

Claims

1. A small-size, high-strength, low-plasticity special wire preparation system, characterized by: The invention comprises a smelting furnace (1), a drainage pipe (3), a cooling device (4), an induction heating device (5), a reel (7), a nitrogen pressure regulating device (9) and an argon filling device (10); an air inlet is arranged at the top of the smelting furnace (1), and the argon filling device (10) is connected to the air inlet via the nitrogen pressure regulating device (9); a discharge port is arranged at the bottom of the smelting furnace (1), and one end of the drainage pipe (3) is connected to the discharge port; the cooling device (4) is used for cooling the drainage pipe (3) and the molten steel therein; the induction heating device (5) is used for heating the wire (8) outputted from the other end of the drainage pipe (3); and the reel (7) is used for reeling the wire (8) heated by the induction heating device (5).

2. The small-size high-strength low-plasticity special wire preparation system according to claim 1 is characterized by: The drainage tube (3) has several models according to the wire specifications.

3. The small-size high-strength low-plasticity special wire preparation system according to claim 1 is characterized by: The cooling device (4) comprises a cooling pipe and a cooling liquid circulation device; the cooling pipe is coiled outside the drainage pipe (3).

4. The small-size high-strength low-plasticity special wire preparation system according to claim 1 is characterized by: It also includes a guide wheel (6); the guide wheel (6) is used to guide the wire (8) heated by the induction heating device (5) to the reel (7).

5. The small-size high-strength low-plasticity special wire preparation system according to any one of claims 1 to 4, characterized in that: The smelting furnace (1) is provided with a pressure sensor; the nitrogen pressure regulating device (9) is provided with a flow control valve and a flow controller; the flow controller regulates the flow control valve through the pressure feedback from the pressure sensor.

6. A method for preparing small-sized high-strength low-plasticity special wire, using the system according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: 1) adding alloy raw materials into a smelting furnace (1) according to the wire material composition requirements, evacuating, heating, and refining until the composition meets the wire material product requirements; 2) filling argon gas into the melting furnace (1), and determining the argon pressure in the melting furnace (1) according to the wire diameter and the finished product winding speed requirements; the argon pressure P in the melting furnace is calculated using the following formula (I); In formula (I), v is the winding rate, mm / min; d is the finished wire diameter, mm; P is the argon filling pressure, Pa; e is a natural constant; 3) The molten steel in the smelting furnace (1) flows into the draft tube (3) under the pressure of argon gas, and is cooled by the cooling device (4) to solidify into wire rod (8); 4) The wire material outputted from the drainage tube (3) is heated by the induction heating device (5) and then rolled up on the winder (7).

7. The method for preparing small-sized high-strength low-plasticity special wire according to claim 6, characterized in that: The drainage tube (3) is replaced with a corresponding model according to the wire material specifications.

8. The method for preparing small-sized high-strength low-plasticity special wire according to claim 6 or 7, characterized in that: In the step 4), the wire is heated by the induction heating device (5) and then guided to the reel (7) through the guide wheel (6).

Citation Information

Patent Citations

  • Equipment and method for hot continuously casting metal wire

    CN101003080A

  • Apparatus for preparing easy-oxidizing hard-distortion alloy wire staff

    CN101157119A

  • Hot continuous casting system

    CN101428337A

  • Semi-continuous casting device and method for magnesium alloy

    CN107030265A

  • Be applied to complex deoxidization device that draws continuous metal cast process

    CN206373332U