Device for preparing aluminum alloy foam special-shaped part through one-step melt transfer and preparation method of aluminum alloy foam special-shaped part
Through a one-step melt transfer preparation method, the Al-Si-Ca-Mg pre-foaming melt was stirred by a crucible resistor furnace and agitator and TiH2 powder was added, and the bottom opening and closing assembly and male mold were combined to perform the compression mold clamping, which solved the aluminum The complex production process and poor stability of alloy foam parts have achieved rapid molding and efficient production, which is suitable for industrial applications.
Patent Information
- Application Number
- CN202411171614.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The production process of aluminum alloy foam special-shaped parts is complex and has poor stability, making it difficult to prepare various special-shaped parts. The traditional foaming method has a long process, a complex process and is seriously wasted.
Using a one-step melt transfer preparation method, the Al-Si-Ca-Mg pre-foaming melt is stirred by heating with a crucible resistor furnace and an electric stirrer. Add TiH2 powder and stir in a foaming barrel. Then the melt is melted through the bottom opening and closing assembly. The body is directly injected into the female mold, and the male mold is combined for block pressing and closing, and the TiH2 is used for foaming and filling.
It greatly reduces the process time, avoids energy waste, simplifies the process, and realizes the rapid molding of aluminum alloy foam special-shaped parts. It has the characteristics of simple process, low cost, high efficiency and environmental protection, and is suitable for large-scale industrial applications.
Smart Images

Figure CN119057041A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparing aluminum alloy foam special-shaped parts, and in particular to a device for preparing aluminum alloy foam special-shaped parts by one-step melt transfer and a preparation method thereof. Background Art
[0002] With the development of the times, in daily life and industry, the requirements for lightweight metal materials are getting higher and higher. The "foam"-like porous structure of aluminum alloy foam determines its use in life and industry.
[0003] Aluminum alloy foam is an excellent structural functional material due to its physical properties such as low density, high specific strength, energy absorption, and sound absorption. Closed-cell aluminum alloy foam exhibits excellent energy absorption performance and higher mechanical damping than aluminum itself. It has been widely used in the production of automotive energy-absorbing blocks, aircraft and ship doors, and other lightweight structural parts that require a certain strength, and has broad application prospects. However, due to the complex production process of foamed aluminum and the control requirements of production process parameters, the product has poor stability and low yield, and it is difficult to prepare various special-shaped parts. Special-shaped parts can only be obtained by molding and cutting using traditional foaming methods. The process is long, the process is complicated, and the waste is serious. How to solve the above problems is an important issue that needs to be solved in the preparation of aluminum alloy foam special-shaped parts. Summary of the invention
[0004] Aiming at the disadvantage that it is difficult to prepare aluminum alloy foam shaped parts, the present invention discloses a method for preparing aluminum alloy foam shaped parts by one-step melt transfer and a preparation device thereof to solve the above problems. Specifically, the present invention proposes a device for preparing aluminum alloy foam shaped parts by one-step melt transfer, comprising: A crucible resistance furnace, wherein the crucible resistance furnace is used to heat the foaming melt; An electric stirrer is located at the upper part of the crucible resistance furnace, and is used to stir the foaming melt and disperse the foaming melt; A foaming barrel, which is located inside the crucible resistance furnace and is used to hold the foaming melt; An asbestos upper cover, which is arranged at the top opening of the crucible resistance furnace and is mainly used to keep the crucible resistance furnace and the foaming barrel warm; A female mold, which is located inside the crucible resistance furnace and at the lower part of the foaming barrel; it is used to receive the foaming melt in the foaming barrel and cooperate with the male mold to prepare special-shaped parts; The support is arranged inside the crucible resistance furnace and is used for supporting the female mold and the foaming barrel.
[0005] Preferably, a stirring rod is provided at the bottom of the electric stirrer, and the stirring rod passes through the asbestos upper cover and extends to the inside of the foaming barrel.
[0006] Preferably, the stirring rod is a TC4 titanium alloy stirring rod.
[0007] Preferably, a bottom opening and closing component for releasing the foaming melt is provided at the bottom of the foaming barrel.
[0008] The opening and closing assembly includes a foaming barrel body and a foaming barrel base fixed at the bottom of the foaming barrel body, and a positioning ring is provided at the bottom of the foaming barrel body for easy connection of the foaming barrel base; the base of the foaming barrel is matched by an operating handle passing through the positioning ring located on the barrel body of the foaming barrel, and the foaming barrel body and the base are clearance-matched when combined.
[0009] Preferably, a temperature-controlling thermocouple for controlling the heating temperature of the crucible resistance furnace is provided at the bottom of the crucible resistance furnace.
[0010] A method for preparing an aluminum alloy foam shaped part by using a device for preparing an aluminum alloy foam shaped part by one-step melt transfer comprises the following steps: S1, heating, heating the temperature in the crucible resistance furnace to 600±5℃; S2, stirring, adding the prepared Al-Si-Ca-Mg pre-foamed melt into the foaming barrel; then adding TiH2 powder into the melt and stirring for 4-6 minutes; S3, melt transfer, open the bottom of the foaming barrel, inject the pre-foamed melt prepared in the foaming barrel directly into the female mold, and take out the foaming barrel; S4, briquetting and pressing. After step S3, briquetting and pressing are performed quickly to make the melt evenly distributed at the bottom of the female mold; S5, closing the male mold. After step S4 is completed, the male mold is quickly pressed to close the mold; S6, foaming and filling, after foaming for 4-6 minutes, the melt is completely filled and distributed between the male mold and the female mold; S7, cooling and demoulding, taking out the molded mold, cooling and molding, and demoulding to obtain the foam aluminum special-shaped part.
[0011] Preferably, in step S2, the temperature in the furnace must be maintained at 600±5°C during stirring.
[0012] Preferably, in step S6, during foaming and filling, the temperature in the crucible resistance furnace must be maintained at 605±5°C.
[0013] Preferably, in step S7, the melt is cooled at a temperature within a range of 15-25°C.
[0014] Compared with the existing technology, the beneficial effect of the present invention is that the device can complete the process of melt preparation and foaming and filling to prepare special-shaped parts in one heating of the crucible resistance furnace, which greatly reduces the process time, avoids energy waste, and is convenient and fast. 2decomposition; at the same time, the bottom opening and closing foaming barrel can use gravity to inject the difficult-to-flow pre-foamed melt into the female mold, avoiding the problem of difficult melt transfer; finally, at the foaming temperature, TiH 2 The powder continuously decomposes and releases H 2 In the process of continuous foaming and filling of the mold, the volume of the molten foam increases rapidly until the mold cavity is completely filled to obtain a completely filled aluminum alloy foam. The present invention has the characteristics of simple process, low cost, high efficiency and environmental protection, and can be applied in large-scale industrial applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is a process flow chart of a device for preparing aluminum alloy foam special-shaped parts by one-step melt transfer proposed by the present invention; Figure 2 A schematic diagram of the overall structure and use process of a device for preparing aluminum alloy foam special-shaped parts by one-step melt transfer proposed by the present invention (section view); Figure 3 This is a structural schematic diagram (three-view drawing) of a foaming barrel body in a device for preparing aluminum alloy foam special-shaped parts by one-step melt transfer proposed by the present invention; Figure 4 It is a structural schematic diagram (three-view drawing) of the bottom of a foaming barrel in a device for preparing aluminum alloy foam shaped parts by one-step melt transfer proposed in an embodiment of the present invention; Figure 5 The figure shows the appearance and hole structure of the foam aluminum special-shaped part prepared by the method in the embodiment of the present invention.
[0016] 1-electric stirrer, 2-asbestos upper cover, 3-TC4 titanium alloy stirring rod, 4-crucible resistance furnace, 5-foaming barrel, 6-female mold, 7-bracket, 8-temperature-controlling thermocouple, 9-pressing block, 10-male mold, 11-foaming melt. DETAILED DESCRIPTION
[0017] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0018] Referring to the drawings, the present invention provides the following device: a device for preparing aluminum alloy foam shaped parts by one-step melt transfer, comprising: A crucible resistance furnace 4, wherein the crucible resistance furnace 4 is used to heat the foaming melt 11; An electric stirrer 1 is located on the upper part of the crucible resistance furnace 4, and the electric stirrer 1 is used to stir the foaming melt 11 and disperse the foaming melt 11; A foaming barrel 5, which is located inside the crucible resistance furnace 4 and is used to contain a foaming melt 11; An asbestos upper cover 2, which is arranged at the top opening of the crucible resistance furnace 4 and is mainly used to keep the crucible resistance furnace 4 and the foaming barrel 5 warm; The female mold 6 is located inside the crucible resistance furnace 4 and at the lower part of the foaming barrel 5; it is used to receive the foaming melt 11 in the foaming barrel 5 and cooperate with the male mold 10 to prepare the special-shaped parts; The support 7 is arranged inside the crucible resistance furnace 4 and is used to support the female mold 6 and the foaming barrel 5 .
[0019] Furthermore, a stirring rod 3 is provided at the bottom of the electric stirrer 1, and the stirring rod 3 passes through the asbestos upper cover and extends to the inside of the foaming barrel.
[0020] Furthermore, the stirring rod 3 is a TC4 titanium alloy stirring rod.
[0021] Furthermore, the bottom of the foaming barrel is provided with a bottom opening and closing component for releasing the foaming melt, such as Figure 3 Figure 4 As shown, the opening and closing assembly includes a foam barrel body 51 and a foam barrel base 52 movably mounted at the bottom of the foam barrel body, and a positioning ring is provided on the bottom side of the foam barrel body 51; the base of the foam barrel is matched by an operating handle passing through the positioning ring located on the barrel body of the foam barrel, and the foam barrel body and the base are clearance-matched when combined. There are two operating handles, one fixed on one side of the barrel body, and the other is fixedly connected to the foam barrel base 52 at the bottom after passing through the positioning ring.
[0022] Furthermore, a temperature-controlling thermocouple for controlling the heating temperature of the crucible resistance furnace is arranged at the bottom of the crucible resistance furnace 4 .
[0023] A method for preparing an aluminum alloy foam shaped part by using a device for preparing an aluminum alloy foam shaped part by one-step melt transfer comprises the following steps: S1, heating, heating the temperature in the crucible resistance furnace to 600±5℃; S2, stirring, adding the prepared Al-Si-Ca-Mg pre-foamed melt into the foaming barrel; then adding TiH2 powder into the melt and stirring for 4-6 minutes; S3, melt transfer, open the bottom of the foaming barrel, inject the pre-foamed melt prepared in the foaming barrel directly into the female mold, and take out the foaming barrel; S4, briquetting and pressing. After step S3, briquetting and pressing are performed quickly to make the melt evenly distributed at the bottom of the female mold; S5, closing the male mold. After step S4 is completed, the male mold is quickly pressed to close the mold; S6, foaming and filling, after foaming for 4-6 minutes, the melt is completely filled and distributed between the male mold and the female mold; S7, cooling and demoulding, taking out the molded mold, cooling and molding, and demoulding to obtain the foam aluminum special-shaped part.
[0024] Preferably, in step S2, the temperature in the furnace must be maintained at 600±5°C during stirring.
[0025] Preferably, in step S6, during foaming and filling, the temperature in the crucible resistance furnace must be maintained at 605±5°C.
[0026] Preferably, in step S7, the melt is cooled at a temperature within a range of 15-25°C.
[0027] In addition, the above embodiments have the following minor differences when implemented: As 1: In an embodiment of the present invention, a method for preparing aluminum alloy foam special-shaped parts by one-step melt transfer specifically comprises the following steps: (1) Melt preparation: Al-Si-Ca-Mg pre-foamed melt is prepared in a foaming barrel based on a method for preparing high-stability aluminum alloy foam. After TiH2 powder is added to the melt, the stirring time is 4-6 minutes, and the temperature in the furnace must be maintained at 600±5℃.
[0028] (2) Melt transfer foaming: Through the bottom opening and closing design of the foaming barrel, the pre-foamed melt prepared in the foaming barrel is directly injected into the female mold, and the melt is quickly evenly distributed on the bottom of the female mold by using a pressing block, and the male mold is quickly closed to keep warm and foam filling. The temperature in the furnace must be maintained at 605±5℃.
[0029] (3) Solidification molding: After foaming for 4-6 minutes, the mold is taken out and cooled to form, and the foamed aluminum special-shaped parts are obtained by demolding.
[0030] Example 2: Compared with Example 1, this example changes the temperature range in the furnace. The detailed steps are as follows: (1) Melt preparation: Al-Si-Ca-Mg pre-foamed melt is prepared in a foaming barrel based on a method for preparing high-stability aluminum alloy foam. After TiH2 powder is added to the melt, the stirring time is 4-6 minutes, and the temperature in the furnace must be maintained at 600±5℃.
[0031] (2) Melt transfer foaming: Through the bottom opening and closing design of the foaming barrel, the pre-foamed melt prepared in the foaming barrel is directly injected into the female mold, and the melt is quickly evenly distributed on the bottom of the female mold by using a pressing block, and the male mold is quickly closed to keep warm and foam filling. The temperature in the furnace must be maintained at 600±5℃.
[0032] (3) Solidification molding: After foaming for 4-6 minutes, the mold is taken out and cooled to form, and the foamed aluminum special-shaped parts are obtained by demolding.
[0033] Example 3: Compared with Example 1, this example changes the foaming time. The detailed steps are as follows: (1) Melt preparation: Al-Si-Ca-Mg pre-foamed melt is prepared in a foaming barrel based on a method for preparing high-stability aluminum alloy foam. After TiH2 powder is added to the melt, the stirring time is 4-6 minutes, and the temperature in the furnace must be maintained at 600±5℃.
[0034] (2) Melt transfer foaming: Through the bottom opening and closing design of the foaming barrel, the pre-foamed melt prepared in the foaming barrel is directly injected into the female mold, and the melt is quickly evenly distributed on the bottom of the female mold by using a pressing block, and the male mold is quickly closed to keep warm and foam filling. The temperature in the furnace must be maintained at 605±5℃.
[0035] (3) Solidification molding: After foaming for 6-8 minutes, the mold is taken out and cooled to form, and the foamed aluminum special-shaped parts are obtained by demolding.
[0036] Example 4: Compared with Example 1, this example changes the method of melt transfer, and the detailed steps are as follows: (1) Melt preparation: (8) Prepare Al-Si-Ca-Mg pre-foamed melt in a foaming barrel based on a method for preparing high-stability aluminum alloy foam. After TiH2 powder is added to the melt, the stirring time is 4-6 minutes, and the temperature in the furnace must be maintained at 600±5℃.
[0037] (2) Melt transfer foaming: Through the hole at the bottom of the foaming barrel, the pre-foamed melt prepared in the foaming barrel is directly injected into the female mold by screw injection, and the melt is quickly evenly distributed at the bottom of the female mold by using a pressing block, and the male mold is quickly closed for heat preservation and foaming filling. The temperature in the furnace must be maintained at 605±5℃.
[0038] (3) Solidification molding: After foaming for 4-6 minutes, the mold is taken out and cooled to form, and the foamed aluminum special-shaped parts are obtained by demolding.
[0039] Example 5: Compared with Example 1, this example changes the type of melt alloy, and the detailed steps are as follows: (4) Melt preparation: Al-Si-Ca-Mg-Sc pre-foamed melt is prepared in a foaming barrel based on a method for preparing high-stability aluminum alloy foam. After TiH2 powder is added to the melt, the stirring time is 4-6 minutes, and the temperature in the furnace must be maintained at 600±5℃.
[0040] (5) Melt transfer foaming: Through the hole at the bottom of the foaming barrel, the pre-foamed melt prepared in the foaming barrel is directly injected into the female mold by screw injection, and the melt is quickly evenly distributed at the bottom of the female mold by using a pressing block, and the male mold is quickly closed for heat preservation and foaming filling. The temperature in the furnace must be maintained at 605±5℃.
[0041] (6) Solidification molding: After foaming for 4-6 minutes, the mold is taken out and cooled to form, and the foamed aluminum special-shaped parts are obtained by demolding.
[0042] The process flow of all embodiments adopts Figure 1 The process flow is shown.
[0043] In the present invention, the melt preparation and foaming and filling process for preparing special-shaped parts can be completed in one heating of the crucible resistance furnace, which greatly reduces the process time, avoids energy waste, and is convenient and fast. After TiH2 decomposition; at the same time, the bottom opening and closing foaming barrel can use gravity to inject the difficult-to-flow pre-foamed melt into the female mold, avoiding the problem of difficult melt transfer; finally, at the foaming temperature, TiH2 powder continuously decomposes to release H2, and the melt foam continuously foams and fills the mold, and the volume of the melt foam grows rapidly until it completely fills the mold cavity, obtaining a completely filled aluminum alloy foam; the present invention has the characteristics of simple process, low cost, high efficiency, and environmental protection, and can be applied in large-scale industrialization.
[0044] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A device for preparing aluminum alloy foam shaped parts by one-step melt transfer, characterized in that: include A crucible resistance furnace, wherein the crucible resistance furnace is used to heat the foaming melt; An electric stirrer is located at the upper part of the crucible resistance furnace, and is used to stir the foaming melt and disperse the foaming melt; A foaming barrel, which is located inside the crucible resistance furnace and is used to hold the foaming melt; An asbestos upper cover, which is arranged at the top opening of the crucible resistance furnace and is mainly used to keep the crucible resistance furnace and the foaming barrel warm; A female mold, which is located inside the crucible resistance furnace and at the lower part of the foaming barrel; it is used to receive the foaming melt in the foaming barrel and cooperate with the male mold to prepare special-shaped parts; The support is arranged inside the crucible resistance furnace and is used for supporting the female mold and the foaming barrel.
2. The device for preparing aluminum alloy foam shaped parts by one-step melt transfer according to claim 1, characterized in that: A stirring rod is arranged at the bottom of the electric stirrer, and the stirring rod passes through the asbestos upper cover and extends to the inside of the foaming barrel.
3. The device for preparing aluminum alloy foam special-shaped parts by one-step melt transfer according to claim 2, characterized in that: The stirring rod is a TC4 titanium alloy stirring rod.
4. The device for preparing aluminum alloy foam shaped parts by one-step melt transfer according to claim 1, characterized in that: A bottom opening and closing assembly for releasing the foaming melt is provided at the bottom of the foaming barrel; the opening and closing assembly includes a foaming barrel body and a foaming barrel base fixed at the bottom of the foaming barrel body; the base of the foaming barrel is matched by an operating handle passing through a positioning ring located on the barrel body of the foaming barrel, and the foaming barrel body and the base are clearance-matched when combined.
5. The device for preparing aluminum alloy foam shaped parts by one-step melt transfer according to claim 1, characterized in that: A temperature-controlling thermocouple for controlling the heating temperature of the crucible resistance furnace is arranged at the bottom of the crucible resistance furnace.
6. A method for preparing aluminum alloy foam shaped parts by using the device for preparing aluminum alloy foam shaped parts by one-step melt transfer according to claim 1, characterized in that: The steps include: S1, heating, heating the temperature in the crucible resistance furnace to 600±5℃; S2, stirring, adding the prepared Al-Si-Ca-Mg pre-foamed melt into the foaming barrel; then adding TiH2 powder into the melt and stirring for 4-6 minutes; S3, melt transfer, open the bottom of the foaming barrel, inject the pre-foamed melt prepared in the foaming barrel directly into the female mold, and take out the foaming barrel; S4, briquetting and pressing. After step S3, briquetting and pressing are performed quickly to make the melt evenly distributed at the bottom of the female mold; S5, closing the male mold. After step S4 is completed, the male mold is quickly pressed to close the mold; S6, foaming and filling, after foaming for 4-6 minutes, the melt is completely filled and distributed between the male mold and the female mold; S7, cooling and demoulding, taking out the molded mold, cooling and molding, and demoulding to obtain the foam aluminum special-shaped part.
7. The method for preparing aluminum alloy foam shaped parts by one-step melt transfer according to claim 6, characterized in that: In step S2, the temperature in the furnace must be maintained at 600±5°C during stirring.
8. The method for preparing aluminum alloy foam shaped parts by one-step melt transfer according to claim 6, characterized in that: In step S4, when using the pressing block, the pressing block needs to be preheated, and the temperature of the pressing block after preheating is 600°C.
9. The method for preparing aluminum alloy foam shaped parts by one-step melt transfer according to claim 6, characterized in that: In step S6, during foaming and filling, the temperature in the crucible resistance furnace must be maintained at 605±5°C.
10. The method for preparing aluminum alloy foam shaped parts by one-step melt transfer according to claim 6, characterized in that: In step S7, the melt is cooled to a temperature of 15-25°C.