Lithium iron phosphate positive electrode material and preparation method thereof

Through the second-stage sintering process of combining rotary kiln and roller kiln, the problems of material loss and low production capacity during the sintering process of lithium iron phosphate positive electrode material are solved, and an efficient sintering process is achieved, which improves electrical performance and cost-effectiveness.

CN119059503APending Publication Date: 2024-12-03NANTONG RESHINE NEW MATERIAL CO LTD

Patent Information

Application Number
CN202310634401.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The lithium iron phosphate positive electrode material has problems such as material loss and low production capacity during the sintering process, which limits its application in the field of high-end electric drives, and the sintering cost is high, which affects the economy of the power battery.

Method used

The second-stage sintering process of combining rotary kiln and roller kiln is adopted. The low-temperature presintering is performed in the rotary kiln to remove waste gas, and then the high-temperature secondary sintering is performed in the roller kiln, and the lithium iron phosphate positive electrode material is obtained through pulverization treatment.

Benefits of technology

It reduces material losses during the sintering process, improves sintering capacity, and improves the electrical performance and cost-effectiveness of the materials. The annual production capacity can reach 45,000 tons/year, the sintering time is reduced by 30%, and the production capacity is increased by 200%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059503A_ABST
    Figure CN119059503A_ABST
Patent Text Reader

Abstract

The invention discloses a lithium iron phosphate positive electrode material and a preparation method thereof, and belongs to the technical field of lithium ion battery positive electrode materials. The preparation method comprises the following steps: firstly, preparing a dry powder material from iron phosphate, a lithium source, a carbon source and an additive, then presintering the dry powder material in a rotary kiln at a first temperature for a first time to obtain a first sintered material, and then secondarily sintering the first sintered material in a roller kiln at a second temperature for a second time to obtain a second sintered material, and finally, crushing the second sintered material to obtain the lithium iron phosphate positive electrode material. Wherein the first temperature is lower than the second temperature, and the first time is shorter than the second time. Sintering is conducted in the mode that low-temperature presintering of the rotary kiln and high-temperature secondary sintering of the roller kiln are combined, reaction produced gas is exhausted during presintering, the problem of material boiling and powder spraying during secondary sintering can be solved, material loss in the sintering process is reduced, and the sintering capacity is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion battery positive electrode materials, in particular to a lithium iron phosphate positive electrode material and a preparation method thereof. Background Art

[0002] As an excellent cathode material for lithium-ion batteries, lithium iron phosphate has an olivine crystal structure. This cathode material has the significant advantages of high safety performance and good cycle performance. However, compared with ternary cathode materials, lithium iron phosphate materials still face the disadvantage of low energy density, which limits their application in the field of high-end electric vehicles. With the emergence of innovative ideas for lithium-ion battery structures in recent years, the blade battery / CTP structure design has been proposed, which has reduced the requirements for material energy density of power batteries, and the application market space of lithium iron phosphate has been further expanded.

[0003] With the large-scale application of lithium-ion batteries, further reducing the cost of power batteries and thus improving the competitive advantage of new energy vehicles has become an important issue. As one of the four main materials of lithium-ion batteries, the cost of cathode materials accounts for more than 35% of the cost of power batteries, and this figure increases with the rise in the price of raw materials such as lithium salts, resulting in huge cost pressure for power battery companies.

[0004] The cost of lithium iron phosphate positive electrode materials mainly includes raw material costs and processing costs. Among the processing costs, sintering costs account for more than 40%. At present, the equipment used for sintering lithium iron phosphate materials in the industry is generally a roller kiln. The sintering method is to load the spray-dried materials into a graphite sagger. As the rollers in the furnace rotate, the sagger is pushed from the furnace head to the furnace tail at a certain speed. During the entire sintering process, the sagger and the materials undergo a process of heating-reaction-exhaust gas discharge-crystallization growth as the temperature curve in the furnace changes. However, during the sintering process, since the material contains about 10% carbon source, a large amount of gas will be generated during sintering. If the material is too full or the heating rate is too fast during sintering, the material in the sagger will boil and overflow a large amount of dust. On the one hand, the dust causes material loss, and on the other hand, it will cause the sintering environment in the furnace to deteriorate and affect the operation and service life of the equipment. Therefore, when lithium iron phosphate is sintered using a roller kiln, it needs to be heated slowly, and the volume of the bowl material can only account for less than 60% of the total volume of the sagger, resulting in low sintering capacity of lithium iron phosphate positive electrode materials. Summary of the invention

[0005] 1. Technical issues to be resolved In view of the deficiencies in the prior art, the present invention provides a lithium iron phosphate positive electrode material and a preparation method thereof, which can reduce material loss during the sintering process of the lithium iron phosphate positive electrode material and improve the sintering capacity.

[0006] (II) Technical solution To achieve the above object, the present invention provides the following technical solutions: A method for preparing a lithium iron phosphate positive electrode material, comprising: The dry powder material is prepared by using iron phosphate, lithium source, carbon source and additives; Pre-sintering the dry powder material in a rotary kiln at a first temperature for a first time to obtain a first sintered material; Secondarily sintering the first sintered material in a roller kiln at a second temperature for a second time to obtain a second sintered material; wherein the first temperature is lower than the second temperature, and the first time is lower than the second time; The second sintered material is crushed to obtain a lithium iron phosphate positive electrode material.

[0007] Optionally, the first temperature is 300-600°C, and the second temperature is 700-800°C.

[0008] Optionally, the first time is 5 to 8 hours, and the second time is 5 to 15 hours.

[0009] Optionally, the pre-sintering is carried out in an inert gas atmosphere. During the pre-sintering, the oxygen concentration in the rotary kiln is within 50 ppm and the furnace pressure is 5 to 40 Pa.

[0010] Optionally, during the pre-sintering, the inclination angle of the rotary kiln is 0.2 to 2 degrees.

[0011] Optionally, the inclination angle of the rotary kiln is 1 degree.

[0012] Optionally, the secondary sintering is carried out in an inert gas atmosphere, and during the second sintering, the oxygen concentration in the roller kiln is within 50 ppm, and the first sintered material is placed in a graphite sagger for the secondary sintering.

[0013] Optionally, the D50 of the dry powder material is 0.3-0.6 μm.

[0014] Optionally, the second sintered material is crushed to a D50 of 0.6 to 1.5 μm to obtain the lithium iron phosphate positive electrode material.

[0015] To achieve the above object, the present invention also provides a lithium iron phosphate positive electrode material prepared by the above preparation method.

[0016] (III) Beneficial effects Compared with the prior art, the present invention provides a lithium iron phosphate positive electrode material and a preparation method thereof, which has the following beneficial effects: 1. The present invention adopts a two-stage sintering process combining a rotary kiln and a roller kiln for sintering, which can reduce material loss during the sintering process and improve sintering capacity. Pre-sintering in a rotary kiln can remove waste gases such as carbon oxides, tar, and VOC gases generated when raw materials such as iron phosphate, lithium source, carbon source, and additives react to obtain pure lithium iron phosphate. The pre-sintering temperature is low, and the increase in magnetic foreign matter generated is very low, which meets the quality control requirements of the product. At the same time, the first sintered material after pre-sintering in the rotary kiln can be cooled by dynamic water cooling, and the cooling rate is high, which is conducive to improving the pre-sintering capacity. According to calculations, the annual production capacity of a single kiln with a diameter of 3m and a length of 40m can reach 45,000 tons / year. In addition, since the waste gas has been discharged during the pre-sintering, the loading amount of the first sintered material can be increased by more than 1.5 times when it is subjected to the secondary sintering in the roller kiln, the sintering time can be reduced by more than 30%, the secondary sintering capacity can be increased by more than 200%, and there will be no problem of material boiling and powder spraying during the sintering process, thereby reducing material losses during the sintering process.

[0017] 2. During the pre-sintering process in the rotary kiln, the material is in dynamic motion and the sintering is highly uniform. When the primary sintered material is subsequently subjected to secondary sintering in a roller kiln at a higher temperature and for a longer time, the physical and chemical properties of the material located in different positions such as the upper layer, middle layer, and lower layer of the same sagger are relatively small, which improves the electrical properties of the final lithium iron phosphate positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work. Among them: Figure 1 It is a schematic flow chart of an embodiment of a method for preparing a lithium iron phosphate positive electrode material of the present invention; Figure 2 This is a state diagram of comparative example 1 before secondary sintering; Figure 3 This is a state diagram of comparative example 1 after secondary sintering; Figure 4 This is a state diagram of comparative example 2 after secondary sintering; Figure 5 This is a state diagram of Example 3 after secondary sintering; Figure 6 It is a comparison chart of the XRD spectra of the materials of Example 1, Example 3 after low-temperature pre-sintering, and Example 3 after secondary sintering. DETAILED DESCRIPTION

[0019] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] See also Figure 1 , Figure 1 It is a schematic flow chart of an embodiment of a method for preparing a lithium iron phosphate positive electrode material of the present invention, and the preparation method comprises the following steps S11-S14.

[0021] Step S11, preparing a dry powder material using iron phosphate, a lithium source, a carbon source and additives.

[0022] The lithium source is a common lithium source in the prior art, such as lithium carbonate, lithium hydroxide, etc. The carbon source is a soluble carbon source such as polyethylene glycol, polyvinyl alcohol, glucose, etc. The additive is a common component in the prior art for other improvement purposes. Specifically, these raw materials required for synthesizing lithium iron phosphate can be configured with water into a slurry with a certain solid content, stirred and dispersed, and then coarsely ground by a sand mill, and part of the coarsely ground slurry is taken for fine grinding, and then mixed with the remaining coarsely ground slurry, so that the D50 of the ground slurry is 0.3-0.6μm, and then spray-dried to obtain the yellow dry powder, which is the above-mentioned dry powder material, and the dry powder material D50 is 10-25μm.

[0023] Step S12, pre-sintering the dry powder material in a rotary kiln at a first temperature for a first time to obtain a first sintered material.

[0024] Then, the dry powder material is pre-sintered at a first temperature in a rotary kiln under an inert gas atmosphere, and the first temperature is 300°C to 600°C, such as 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, etc. During the pre-sintering, the oxygen concentration inside the rotary kiln is greater than 0 and less than or equal to 50ppm, such as 5ppm, 10ppm, 15ppm, 20ppm, 30ppm, 40ppm, etc., the furnace pressure is 5-40Pa, such as 5Pa, 10Pa, 15Pa, 20Pa, 25Pa, 30Pa, 35Pa, 40Pa, etc., and the inclination angle of the rotary kiln is 0.2-2 degrees, such as 0.2 degrees, 0.5 degrees, 0.8 degrees, 1 degree, 1.3 degrees, 1.5 degrees, 1.8 degrees, 2 degrees, etc. The first time for pre-sintering the material in the rotary kiln is 5 to 8 hours, for example, 5 hours, 5.5 hours, 6 hours, 6.5 hours, 7 hours, 7.5 hours, 8 hours, etc., to obtain a first sintered material.

[0025] When the dry powder material is pre-sintered at the first temperature, the carbon source decomposes to produce organic gas. Under the action of the organic gas, the iron phosphate and the lithium source can react quickly to generate pure lithium iron phosphate. Under the conditions of the first temperature and the first time set by the present invention, the carbon source and the lithium source react completely, and no by-product waste gas is generated during the subsequent secondary sintering. The selection of the inclination angle of the rotary kiln is conducive to promoting the reaction during the pre-sintering process, ensuring that the reaction is carried out thoroughly, and is also conducive to the uniformity of the reaction, so that all parts of the material react thoroughly.

[0026] Step S13, re-sintering the first sintered material in a roller kiln at a second temperature for a second time to obtain a second sintered material; wherein the first temperature is lower than the second temperature, and the first time is lower than the second time.

[0027] This step is to load the first sintered material into a graphite crucible, and use a roller kiln to perform high-temperature secondary sintering in an inert gas atmosphere, and the sintering temperature is 700-800°C, for example, 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, etc. During the second sintering, the oxygen concentration in the roller kiln is greater than 0 and less than or equal to 10ppm, for example, 1ppm, 3ppm, 5ppm, 7ppm, 9ppm. The second time for the material to be sintered in the roller kiln is 5-15 hours, for example, 5 hours, 6 hours, 7 hours, 8 hours, 10 hours, 12 hours, 15 hours, etc., to obtain the second sintered material.

[0028] Step S14, crushing the second sintered material to obtain a lithium iron phosphate positive electrode material.

[0029] Specifically, the second pulverized material can be pulverized by pulverizing equipment such as a jet mill commonly used in the prior art to obtain the lithium iron phosphate positive electrode material.

[0030] This embodiment first uses a rotary kiln for pre-sintering, which can remove waste gases such as carbon oxides, tar, VOC gases, etc. produced when raw materials such as iron phosphate, lithium source, carbon source and additives react, and obtain pure lithium iron phosphate at the same time. The pre-sintering temperature is low, and the increment of magnetic foreign matter produced is very low, which meets the quality control requirements of the product. When the subsequent secondary sintering with higher temperature and longer time is carried out, since the waste gas has been discharged during the pre-sintering, the loading capacity of the roller kiln can be increased by more than 1.5 times, the sintering time is reduced by more than 30%, and the secondary sintering capacity is increased by more than 200%, and the problem of material boiling and powder spraying will not occur during the secondary sintering process, thereby reducing the material loss during the sintering process. Moreover, during the pre-sintering process of the rotary kiln, the material is in dynamic motion, and the sintering uniformity is high. When the primary sintered material is subsequently subjected to secondary sintering, the physical and chemical properties of the materials located in different positions such as the upper layer, middle layer, and lower layer in the same sagger are relatively small, so that the electrical properties of the lithium iron phosphate positive electrode material finally obtained are improved.

[0031] Based on the same inventive concept, the present invention also provides a lithium iron phosphate positive electrode material, which is prepared by the preparation method described in the above embodiment and has the same beneficial effects as the above embodiment, which will not be repeated here.

[0032] The beneficial effects of the present invention are described below by means of specific comparative examples and embodiments.

[0033] Comparative Example 1 The lithium iron phosphate positive electrode material prepared by the following steps is recorded as Comparative Example 1: (1) Weigh 50 kg of iron phosphate, 12.36 kg of lithium carbonate, 6.07 kg of glucose, 87.46 g of TiO2 and 187.14 g of V2O5 as additives, add the above raw materials into 90 kg of pure water, and stir with a paddle stirrer for 30 minutes; (2) The slurry after stirring and dispersion was ground to D50 = 1.45 μm using a sand mill (coarse grinding, zirconium bead diameter 0.6 mm) to obtain slurry J1, and then 79.2 kg (accounting for 50% of the total volume of the slurry) was taken out from the J1 slurry and transferred to the fine grinding system for fine grinding to D50 = 0.35-0.40 μm to obtain slurry J2, and then the remaining J1 slurry and J2 slurry were transferred to a mixing tank for stirring and mixing for 30 minutes to obtain slurry J3, and the D50 of slurry J3 was 1.0 μm; (3) The slurry J3 is dried using a spray dryer to obtain a dry powder material J4. The dry powder material has a D50 of 10-25 μm and a moisture content of about 2%.

[0034] (4) The dry powder material J4 was loaded into a graphite sagger and sintered in a roller kiln. The sagger size was 330 mm*330 mm*220 mm. The bulk density of the dry powder material J4 was about 0.65 g / cc. The loading amount was 12 kg. The sagger volume filling rate was about 90.0%. The material was first heated to 740°C at a heating rate of 5°C / min under a nitrogen atmosphere and kept warm for 8 hours to obtain a sintered material. (5) The sintered material is crushed using a jet mill to obtain the lithium iron phosphate positive electrode material of Comparative Example 1.

[0035] Comparative Example 2: The difference from Comparative Example 1 is that the amount of dry powder material J4 loaded in the sagger is 8 kg, the sagger volume filling rate is about 60.1%, and the roller kiln is first heated to 740°C at a heating rate of 3°C / min. The rest of the processes are the same, and the lithium iron phosphate positive electrode material of Comparative Example 2 is obtained.

[0036] The above comparative examples 1 and 2 both adopt the traditional sintering process, and the following embodiments adopt the segmented secondary sintering process of low-temperature pre-sintering and high-temperature secondary sintering provided by the present invention. Example

[0037] The lithium iron phosphate positive electrode material prepared by the following steps is recorded as Example 1: (1) The dry powder material J4 was obtained according to the same process as in Comparative Example 1; (2) The dry powder material J4 is put into a rotary kiln for pre-sintering. The first pre-sintering temperature is 450°C. Nitrogen protective gas is introduced. The oxygen concentration in the rotary kiln is about 8ppm. The sintering furnace pressure is 23pa. The inclination angle of the rotary kiln is 1 degree. During the whole pre-sintering process, the material stays in the rotary kiln for 6 hours. A cooling kiln is arranged behind the rotary kiln. The rotary kiln body is cooled by spraying cooling water. After cooling, the material is collected in a ton bag to obtain the first sintered material S1. (3) The first sintered material S1 is loaded into a graphite sagger and sent into a rotary kiln for secondary sintering. The sagger size is 330 mm*330 mm*220 mm. The bulk density of the first sintered material S1 is about 0.83 g / cc. The loading amount is 12 kg. The sagger volume filling rate is about 70.7%. The material is first heated to 740°C at a heating rate of 5°C / min under a nitrogen atmosphere and kept warm for 8 hours, i.e., the second time of the secondary sintering is 8 hours, to obtain a second sintered material S2. (4) The second sintered material S2 is crushed by using a jet mill to obtain the lithium iron phosphate positive electrode material of Example 1.

[0038] Example 2: The difference from Example 1 is that the amount of the sagger filled is 14 kg, the volume filling rate of the sagger is about 82.5%, the second time of the secondary sintering is 6 hours, and the other processes are the same to obtain the lithium iron phosphate positive electrode material of Example 2.

[0039] Example 3: The difference from Example 1 is that the amount of the sagger filled is 15 kg, the sagger filling rate is about 88%, the second time of the secondary sintering is 6 hours, and the other processes are the same to obtain the lithium iron phosphate positive electrode material of Example 3.

[0040] See also Figure 2-Figure 5 , Figure 2 This is a photo of the state before sintering of Comparative Example 1. Figure 3 and Figure 4 They are photos of the sintered state of Comparative Example 1 and Comparative Example 2, Figure 5The state photo after the secondary sintering of Example 3 shows that in the traditional sintering process of Comparative Example 1, under the potting amount and heating rate of Comparative Example 1, there is a serious powder spraying situation. If the material loss and the impact on the equipment caused by this phenomenon are to be alleviated, measures such as reducing the potting amount and reducing the heating rate must be taken, such as the case of Comparative Example 2, which will inevitably lead to too low production capacity; and using the preparation process provided by the present invention, the material after pre-sintering in the rotary kiln, Example 1, Example 2, especially Example 3, under high potting amount and high heating rate, there is basically no problem of material boiling and powder spraying in the secondary sintering process in the roller kiln, indicating that the present invention can reduce material loss in the sintering process and improve sintering capacity at the same time. The specific capacity comparison is shown in Table 1 below, and it can be seen that the capacity brought by the technical solution of the present invention is significantly improved.

[0041]

[0042] Recombination Figure 6 Come and see, Figure 6 The three XRD curves from bottom to top correspond to the positive electrode material of Example 1, the first sintered material S1 obtained by low temperature pre-sintering in Example 3, and the positive electrode material of Example 3. It can be seen from the XRD diagram that after the dry powder material was pre-sintered at 450°C in a rotary kiln, a pure-phase olivine-type lithium iron phosphate structure has been formed. After secondary sintering at 740°C, the crystalline phase is maintained, which is consistent with the crystalline phase obtained by the traditional sintering process.

[0043] Furthermore, the lithium iron phosphate positive electrode materials of the above comparative examples and embodiments were made into batteries and then tested for key technical indicators such as charge and discharge capacity. The test results are shown in Table 2 below.

[0044]

[0045] It can be seen from the data in Table 2 above that the low-temperature discharge capacity of each embodiment of the present invention exceeds 60, which is significantly higher than that of Comparative Example 1 and Comparative Example 2. The 0.1C charging capacity, 0.1C discharge capacity, and 1C discharge capacity of Examples 1-3 are all better than those of Comparative Example 1 and Comparative Example 2.

[0046] After low-temperature pretreatment in a rotary kiln, the performance of the lithium iron phosphate positive electrode material obtained in Example 3 under the sintering conditions of a loading amount of 15 kg and a secondary sintering time of 6 hours is still better than that of the lithium iron phosphate positive electrode materials of Comparative Examples 1 and 2 under traditional process conditions, indicating that the preparation method provided by the present invention can obtain a higher loading amount and a shorter sintering time, while improving production capacity and maintaining the excellent electrochemical properties of the material.

[0047] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a lithium iron phosphate positive electrode material, It is characterized in that include: The dry powder material is prepared by using iron phosphate, lithium source, carbon source and additives; Pre-sintering the dry powder material in a rotary kiln at a first temperature for a first time to obtain a first sintered material; Secondarily sintering the first sintered material in a roller kiln at a second temperature for a second time to obtain a second sintered material; wherein the first temperature is lower than the second temperature, and the first time is lower than the second time; The second sintered material is crushed to obtain a lithium iron phosphate positive electrode material.

2. The preparation method according to claim 1, It is characterized in that The first temperature is 300-600°C, and the second temperature is 700-800°C.

3. The preparation method according to claim 2, It is characterized in that The first time is 5 to 8 hours, and the second time is 5 to 15 hours.

4. The preparation method according to claim 1, It is characterized in that The pre-sintering is carried out in an inert gas atmosphere. During the pre-sintering, the oxygen concentration in the rotary kiln is within 50 ppm and the furnace pressure is 5-40 Pa.

5. The preparation method according to claim 4, It is characterized in that During the pre-sintering, the inclination angle of the rotary kiln is 0.2 to 2 degrees.

6. The preparation method according to claim 5, It is characterized in that The inclination angle of the rotary kiln is 1 degree.

7. The preparation method according to claim 1, It is characterized in that The secondary sintering is carried out in an inert gas atmosphere. When the second sintering is carried out, the oxygen concentration in the roller kiln is within 50 ppm. The first sintering material is placed in a graphite sagger for the secondary sintering.

8. The preparation method according to claim 1, It is characterized in that The D50 of the dry powder material is 0.3-0.6 μm.

9. The preparation method according to claim 8, It is characterized in that The second sintered material is crushed to a D50 of 0.6-1.5 μm to obtain the lithium iron phosphate positive electrode material.

10. A lithium iron phosphate positive electrode material, It is characterized in that The lithium iron phosphate positive electrode material is prepared according to the preparation method according to any one of claims 1-9.

Citation Information

Patent Citations

  • Preparation method of lithium iron phosphate cathode material

    CN111146439A

  • Preparation method of high-nickel ternary positive electrode material for lithium ion battery

    CN112125353A

  • Efficient lithium iron phosphate sintering method for improving carbon coating effect

    CN115849323A

  • Method for preparing lithium iron phosphate positive electrode material

    CN115924876A

  • Method for preparing high-performance lithium iron phosphate through segmented sintering

    CN115959644A

Cited By

  • Positive electrode active material and low-cost preparation method therefor, secondary battery, and electrical device

    WO2026138010A1