Preparation method of lithium ion energy storage negative electrode material with long service life and low cost

By carbonizing natural graphite spherical tail material and hard carbon precursor at high temperature and grafting polymers on its surface, the problem of poor circulation stability of the negative electrode material of potassium ion battery is solved, and the high-magnification long cycle of lithium ion battery is achieved and excellent cycle stability, suitable for large-scale production.

CN119059518AInactive Publication Date: 2024-12-03SHENZHEN GUANGFENG NEW ENERGY TECH INNOVATION CENT CO LTD

Patent Information

Application Number
CN202411183445.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The cyclic stability and unsatisfactory performance of the negative electrode materials of existing potassium ion batteries are poor, and the synthesis process of most modification methods is cumbersome and the raw material cost is high, which increases the difficulty of commercializing potassium ion batteries.

Method used

The high-temperature carbonization is carried out using natural graphite spherical tail material and hard carbon precursor, and polymer and catalyst are added on it. High-performance, low-cost lithium-ion battery negative electrode material is prepared through oxidation treatment and grafting reaction to realize the battery High magnification long cycles and excellent cycle stability during charge and discharge.

Benefits of technology

It realizes high magnification and long cycles of lithium-ion batteries during charging and discharging, and has excellent cycle stability, simple operation, suitable for large-scale production, and is suitable for two or more types of battery negative electrode systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059518A_ABST
    Figure CN119059518A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a long-life low-cost lithium ion energy storage negative electrode material, which comprises the following steps: taking a certain mass of purified natural graphite spherical tailings, adding a certain amount of oxidant, and stirring at room temperature for 2-8 hours for oxidation treatment to obtain a product 1; uniformly mixing the product 1 and a hard carbon precursor according to a certain proportion, carrying out high-temperature carbonization at a specific temperature, and carrying out heat preservation for a period of time to obtain a product 2; respectively dissolving a plurality of first polymers in a solvent, mixing, and stirring at a certain temperature for a period of time to obtain a product 3; mixing, stirring and grafting the product 2 and the product 3 to obtain a mixed solution, then adding a second polymer into the mixed solution, stirring for 6 hours at 60 DEG C, and dialyzing and drying the mixed solution to obtain a final product. The material realizes high-rate long circulation of the battery in the charge-discharge process, has excellent circulation stability, is simple to operate and is suitable for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a method for preparing a long-life, low-cost lithium ion energy storage negative electrode material. Background Art

[0002] As energy storage devices, lithium-ion batteries (LIBs) have been widely used in portable electronic devices and electric vehicles, and the technology is relatively mature. Among the negative electrode materials of lithium-ion batteries, natural graphite is widely used due to its low cost and good electrochemical properties. The cycle life of natural graphite negative electrode is the core of energy storage materials. In order to further reduce the cost of energy storage, it is necessary to modify natural graphite to increase its cycle life.

[0003] At the same time, potassium-ion batteries (PIBs) are the most promising alternative to lithium-ion batteries because of their many potential advantages, including (1) the abundance and low cost of potassium metal resources; (2) the standard redox potential of potassium-ion batteries (±2.92 V vs. SHE) is comparable to that of lithium-ion batteries (±3.04 V vs. SHE), indicating that they have a higher battery voltage; and (3) the conductivity of potassium-ion battery electrolytes is higher than that of lithium-ion batteries.

[0004] Graphite materials can be used not only in lithium-ion batteries, but also provide relatively high specific capacity (279 mA h g-1) and low average insertion potential (≈0.1 V) for potassium-ion batteries. However, due to the ionic radius of potassium Much larger than the ionic radius of lithium When potassium ions are inserted into the graphite layer, the interlayer spacing of the graphite lattice will expand to Therefore, when natural graphite is used as the negative electrode material of potassium ion batteries, the huge volume change (≈61%) irreversibly destroys the solid electrolyte layer (SEI). At the same time, the slow diffusion dynamics of potassium ions in the graphite layer lead to poor cycle stability and unsatisfactory rate performance.

[0005] To solve this problem, researchers have made a lot of attempts, but most of them have problems with cumbersome synthesis process and high raw material costs, which greatly increases the difficulty of commercializing potassium ion batteries.

[0006] Therefore, there is an urgent need to provide a method for preparing a long-life, low-cost lithium-ion energy storage negative electrode material to solve the above problems. Summary of the invention

[0007] The purpose of the present invention is to overcome the shortcomings and defects of the prior art and provide a method for preparing a long-life, low-cost lithium-ion energy storage negative electrode material, so as to achieve a high-rate long cycle of the battery during the charge and discharge process, and at the same time have excellent cycle stability, simple operation, and be suitable for large-scale production.

[0008] The objective of the present invention is achieved through the following technical solutions:

[0009] A method for preparing a long-life, low-cost lithium-ion energy storage negative electrode material comprises the following steps:

[0010] Step 1, taking a certain mass of purified natural graphite spherical tailings, adding a certain amount of oxidant, stirring at room temperature for 2-8 hours for oxidation treatment, to obtain product 1;

[0011] Step 2, mixing the product 1 and the hard carbon precursor in a certain proportion, and carbonizing them at a specific temperature, and then keeping them warm for a period of time to obtain the product 2;

[0012] Step 3, dissolving a plurality of first polymers in a solvent respectively, mixing and stirring at a certain temperature for a period of time to obtain a product 3;

[0013] Step 4: Mix product 2 and product 3 and stir them for grafting to obtain a mixed solution, then add the second polymer to the mixed solution, stir at 60° C. for 6 hours, dialyze the mixed solution, and dry it to obtain the final product.

[0014] As a preferred technical solution of the present invention, the particle size D50 of the natural graphite spherical tailings in step 1 is 0.5 μm to 10 μm, and the fixed carbon content in the purified natural graphite spherical tailings is greater than 99%.

[0015] As a preferred technical solution of the present invention, the solid-liquid ratio of the natural graphite spherical tailings to the oxidant in step 1 is 5:1 to 1:50, and the oxidant is one or a combination of two or more of hydrogen peroxide, concentrated nitric acid, concentrated sulfuric acid, concentrated hydrochloric acid, potassium hydroxide, and potassium permanganate.

[0016] As a preferred technical solution of the present invention, the hard carbon precursor is one or a combination of two or more of glucose, biomass tar, phenolic resin, polyvinyl pyrrolidone, citric acid, high-sulfur coal, lignite, and coking coal.

[0017] As a preferred technical solution of the present invention, the mass ratio of the product 1 in step 2 to the hard carbon precursor is 100:5-100:50, the carbonization temperature is 500-1500° C., and the insulation time is 2-6 hours.

[0018] As a preferred technical solution of the present invention, the product 1 and the hard carbon precursor in step 2 need to be carbonized at high temperature under the protection of a carburizing atmosphere, and the carburizing atmosphere is any one of an argon atmosphere, a nitrogen atmosphere, and a hydrogen-argon mixed atmosphere, wherein the hydrogen in the hydrogen-argon mixed atmosphere accounts for 5%.

[0019] As a preferred technical solution of the present invention, the first polymer in step 3 is a combination of two or more of polyacrylic acid, tannic acid, carboxymethyl cellulose, KH550, KH560, phosphoric acid, thermoplastic polyurethane, phytic acid, polyetheramine, tannic acid, polyvinyl alcohol, dopamine, sodium alginate, glutaraldehyde, and chitosan.

[0020] As a preferred technical solution of the present invention, in step 3, the reaction temperature of the multiple first polymers is 30-100° C., and the stirring time is 2-12 h.

[0021] As a preferred technical solution of the present invention, the second polymer in step 4 is one or a combination of two of β-cyclodextrin, polyvinyl pyrrolidone, water-soluble starch, guar gum, xanthan gum, and glucose.

[0022] As a preferred technical solution of the present invention, in step 4, the reaction time of mixing and stirring the product 2 and the product 3 to graft the active material is 10-24 hours.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The present invention uses natural graphite spherical tailings and hard carbon precursors as raw materials, performs high-temperature carbonization on the oxidized natural graphite spherical tailings and a certain proportion of hard carbon precursors, adds high-molecular polymers and catalysts thereon, and after a period of reaction, centrifuges, washes, and filtrates to obtain high-performance, low-cost battery negative electrode materials. The battery can achieve high-rate long cycles during the charge and discharge process, and has excellent cycle stability. The preparation method of the present invention is simple to operate, suitable for large-scale production, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a structural schematic diagram of the present invention.

[0026] Figure 2 Figure 2 shows the charge and discharge cycle test diagram of (a) lithium-ion battery and (b) potassium-ion battery.

[0027] Figure 3 These are rate performance test diagrams of (a) lithium-ion batteries and (b) potassium-ion batteries. DETAILED DESCRIPTION

[0028] The present invention is further described in detail below in conjunction with the examples and drawings, but the embodiments of the present invention are not limited thereto. The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.

[0029] The specific implementation process of the present invention is as follows:

[0030] A method for preparing a long-life, low-cost lithium-ion energy storage negative electrode material comprises the following steps:

[0031] Step 1, taking a certain mass of purified natural graphite spherical tailings, adding a certain amount of oxidant, stirring at room temperature for 2-8 hours for oxidation treatment, to obtain product 1;

[0032] Step 2, mixing the product 1 and the hard carbon precursor in a certain proportion, and carbonizing them at a specific temperature, and then keeping them warm for a period of time to obtain the product 2;

[0033] Step 3, dissolving a plurality of first polymers in a solvent respectively, mixing and stirring at a certain temperature for a period of time to obtain a product 3;

[0034] Step 4, mix and stir product 2 and product 3 to obtain a mixed solution, then add the second polymer to the mixed solution, stir for 6 hours at 60°C, dialyze the mixed solution, and dry to obtain the final product. Specifically, product 1 is graphite after oxidation, and product 2 is a composite material after carbonization. The present invention uses natural graphite spherical tailings and hard carbon precursors as raw materials for secondary granulation, and utilizes the chaotic layer structure and pores of the hard carbon material to achieve rapid and stable transmission of Li+ and K+, so that it has a higher capacity retention rate at high current density. By grafting a high molecular polymer on the surface of the isotropic structure, the solvent is prevented from being co-embedded in the natural graphite, thereby improving the cycle stability of the negative electrode.

[0035] The composite material with multiple layers and multiple voids is obtained by secondary granulation of natural graphite spherical tailings and hard carbon precursors, and polymers are grafted on the surface. By selecting different hard carbons and polymers, the structural stability and rate performance of the negative electrode material are improved. In the cycle process, it can not only buffer the volume change caused by charging and discharging, but also stabilize SEI, thereby obtaining a high-rate and long-cycle lithium-ion negative electrode material, which can be used for two or more types of battery negative electrode systems. At the same time, the natural graphite spherical tailings are used as solid waste for high value utilization.

[0036] The present invention will be further described below in conjunction with specific embodiments.

[0037] Example 1

[0038] A certain amount of purified natural graphite spherical tailings was placed in 30% hydrogen peroxide with a solid-liquid ratio of 1:5, magnetically stirred for 4 hours, rinsed with deionized water, filtered and dried to obtain oxidized graphite. Then it was ground and mixed with a certain amount of biomass tar, placed in a nitrogen-filled tubular furnace for high-temperature carbonization at 900°C, and kept warm for 3 hours to obtain a carbonized composite material. In the methanol solution of polyetheramine, an equimolar number of KH560 was added, and stirred in a water bath at 50°C for 12 hours to obtain product 3. Then the carbonized composite material was added to product 3 and stirred for 12 hours to obtain a mixed solution, and then an excess of polyvinyl pyrrolidone was added to the mixed solution, magnetically stirred at 60°C for 6 hours, and the mixed solution was dialyzed and freeze-dried to obtain a hard carbon composite material.

[0039] The hard carbon composite material prepared above is directly used as the negative electrode material of lithium-ion battery, with metal lithium sheet or metal potassium sheet as the counter electrode, Celgard2325 as the separator, 1mol / L LiPF6 as the electrolyte, wherein the volume ratio of LiPF6 solvent is 1:1 ethylene carbonate and dimethyl carbonate mixed liquid, and assembled into CR2032 type button battery in an argon-protected glove box. The voltage charge and discharge range in the blue electricity test is 0.01~3V. Figure 2 The charge and discharge cycle test diagrams of (a) lithium-ion batteries and (b) potassium-ion batteries show that the lithium-ion battery exhibits a specific capacity of 244.9 mAh / g after 1000 cycles at a current density of 1 A / g, and the potassium-ion battery exhibits a specific capacity of 136.8 mA h / g after 250 cycles at a current density of 0.1 A / g. Figure 3 Figure 1 is a rate performance test diagram of (a) lithium-ion battery and (b) potassium-ion battery. In the test program, the charge and discharge current density of the lithium-ion battery is 0.1A / g, 0.2A / g, 0.5A / g, 1.0A / g, 2.0A / g, 5.0A / g, 2.0A / g, 1.0A / g, 0.5A / g, 0.2A / g, 0.1A / g, and the charge and discharge density of the potassium-ion battery is 0.05A / g, 0.1A / g, 0.2A / g, 0.5A / g, 1.0A / g, 0.5A / g, 0.2A / g, 0.1A / g, 0.05A / g. The number of charge and discharge cycles at the same current density is 10. The specific capacity of the lithium-ion battery before and after adding hard carbon at a current density of 5.0A / g is 27.6mA h / g and 121.4mA h / g, respectively. h / g. The specific capacities of potassium ion batteries before and after adding hard carbon at a current density of 1.0A / g were 9.2mA h / g and 80.9mAh / g, respectively. In comparison, it can be clearly seen that after adding hard carbon, better rate performance was obtained under different current densities. The modified negative electrode material showed higher capacity and cycle stability.

[0040] Example 2

[0041] A certain mass of purified natural graphite spherical tailings was placed in 30% concentrated sulfuric acid with a solid-liquid ratio of 1:5, magnetically stirred for 4 hours, rinsed with deionized water, filtered and dried to obtain oxidized graphite. Then it was ground and mixed with a certain mass of biomass tar, placed in a tubular furnace filled with argon for high-temperature carbonization at 900°C, and kept warm for 3 hours to obtain a carbonized composite material. Dopamine was dissolved in a buffer solution and mixed evenly, and then an equimolar number of KH560 was added, wherein the buffer solution can be an acetate buffer solution, a phosphate buffer solution, a Tris hydrochloric acid buffer solution and a BR buffer solution, and stirred in a water bath at 40°C for 12 hours to obtain product 3. Then the carbonized composite material was added to product 3 and stirred for 12 hours to obtain a mixed solution, and then an excess of xanthan gum was added to the solution, magnetically stirred at 60°C for 6 hours, and the mixed solution was dialyzed and freeze-dried to obtain a hard carbon composite material. The final material was assembled into a semi-button battery for charge and discharge performance testing. Figure 2 It shows that the lithium-ion battery exhibits a specific capacity of 245.7 mA h / g after 1000 cycles at a current density of 1 A / g, and the potassium-ion battery exhibits a specific capacity of 137.2 mA h / g after 250 cycles at a current density of 0.1 A / g. Figure 3 It shows that the specific capacity of lithium-ion batteries before and after adding hard carbon at a current density of 5.0A / g was 26.9mA h / g and 122.4mA h / g respectively, and the specific capacity of potassium-ion batteries before and after adding hard carbon at a current density of 1.0A / g was 9.6mA h / g and 79.3mA h / g respectively. In comparison, it can be clearly seen that after adding hard carbon, better rate performance is obtained under different current densities, and the modified negative electrode material shows higher capacity and cycle stability.

[0042] Example 3

[0043] A certain amount of purified natural graphite spherical tailings were placed in 10% potassium hydroxide with a solid-liquid ratio of 2:3, magnetically stirred for 4 hours, rinsed with deionized water, filtered and dried to obtain oxidized graphite. Then it was mixed with a certain amount of ethanol solution of phenolic resin, stirred at room temperature for 1 hour, and the ethanol solution was slowly evaporated at 70°C. Under the protection of nitrogen atmosphere, the obtained product was cured at 100°C for 1 hour, and then heated to 900°C at a heating rate of 2°C / min for carbonization for 3 hours to obtain a carbonized composite material. 1g of glutaraldehyde was dissolved in 33mL of 2wt% acetic acid aqueous solution and mixed evenly, and an equal molar number of KH550 was added and stirred for 5 hours to obtain product 3. Then the carbonized composite material was added to product 3 and stirred for 12 hours to obtain a mixed solution, and then an excess of chitosan was added to the solution, magnetically stirred at 60°C for 6 hours, and the mixed solution was dialyzed and dried at 80°C to obtain a hard carbon composite material. The final material was assembled into a semi-button battery for charge and discharge performance testing. Figure 2 It shows that the lithium-ion battery exhibits a specific capacity of 246.3 mA h / g after 1000 cycles at a current density of 1 A / g, and the potassium-ion battery exhibits a specific capacity of 137.5 mA h / g after 250 cycles at a current density of 0.1 A / g. Figure 3 It shows that the specific capacity of lithium-ion batteries before and after adding hard carbon at a current density of 5.0A / g is 27.13mA h / g and 122.1mA h / g respectively, and the specific capacity of potassium-ion batteries before and after adding hard carbon at a current density of 1.0A / g is 9.4mA h / g and 80.16mA h / g respectively. In comparison, it can be clearly seen that after adding hard carbon, better rate performance is obtained under different current densities, and the modified negative electrode material shows higher capacity and cycle stability.

[0044] Example 4

[0045] A certain mass of purified natural graphite spherical tailings was placed in 20% potassium permanganate with a solid-liquid ratio of 1:2, magnetically stirred for 4 hours, rinsed with deionized water, filtered and dried to obtain oxidized graphite. Then it was mixed with a certain mass of ethanol solution of phenolic resin, stirred at room temperature for 1 hour, and the ethanol solution was slowly evaporated at 70°C. Under the protection of nitrogen atmosphere, the obtained product was cured at 100°C for 1 hour, and then heated to 900°C at a heating rate of 2°C / min for carbonization for 3 hours to obtain a carbonized composite material. Tannic acid and KH550 with a mass ratio of 1:8 were dissolved in water and mixed evenly, and stirred in a water bath at 80°C for 5 hours to obtain product 3. Then the carbonized composite material was added to product 3 and stirred for 12 hours to obtain a mixed solution, and then an excess of β-cyclodextrin reagent was added to the solution, magnetically stirred at 60°C for 6 hours, and the mixed solution was dialyzed and freeze-dried to obtain a hard carbon composite material. The final material was assembled into a semi-button battery for charge and discharge performance testing. Figure 2It shows that the lithium-ion battery exhibits a specific capacity of 244.89 mA h / g after 1000 cycles at a current density of 1 A / g, and the potassium-ion battery exhibits a specific capacity of 138.11 mA h / g after 250 cycles at a current density of 0.1 A / g. Figure 3 It shows that the specific capacity of lithium-ion batteries before and after adding hard carbon at a current density of 5.0A / g is 27.1mA h / g and 123.41mA h / g respectively, and the specific capacity of potassium-ion batteries before and after adding hard carbon at a current density of 1.0A / g is 10.2mA h / g and 81.4mA h / g respectively. In comparison, it can be clearly seen that after adding hard carbon, better rate performance is obtained under different current densities, and the modified negative electrode material shows higher capacity and cycle stability.

[0046] Example 5

[0047] A certain amount of purified natural graphite spherical tailings was placed in 10% potassium hydroxide with a solid-liquid ratio of 1:5, magnetically stirred for 4 hours, rinsed with deionized water, filtered and dried to obtain oxidized graphite. Then it was mixed with a certain amount of citric acid and ammonium chloride aqueous solution, stirred at room temperature for 5 hours, freeze-dried for 48 hours, and pyrolyzed at 800°C for 2 hours under argon atmosphere protection to obtain a carbonized composite material. Carboxymethyl cellulose (CMC) was dissolved in water and stirred overnight to obtain a 50%wt viscous solution. An equal number of moles of KH560 was added to the solution, and stirred in a water bath at 60°C for 5 hours to obtain product 3. The carbonized composite material was then added to product 3 and stirred for 12 hours to obtain a mixed solution. Subsequently, an excess of soluble starch reagent was added to the solution, magnetically stirred at 60°C for 6 hours, and the mixed solution was dialyzed and freeze-dried to obtain a hard carbon composite material. The final material was assembled into a semi-button battery for charge and discharge performance testing. Figure 2 It shows that the lithium-ion battery exhibits a specific capacity of 243.85 mA h / g after 1000 cycles at a current density of 1 A / g, and the potassium-ion battery exhibits a specific capacity of 135.88 mA h / g after 250 cycles at a current density of 0.1 A / g. Figure 3 It shows that the specific capacity of lithium-ion batteries before and after adding hard carbon at a current density of 5.0A / g is 27.56mA h / g and 120.96mA h / g respectively, and the specific capacity of potassium-ion batteries before and after adding hard carbon at a current density of 1.0A / g is 11.52mA h / g and 80.44mA h / g respectively. In comparison, it can be clearly seen that after adding hard carbon, better rate performance is obtained under different current densities, and the modified negative electrode material shows higher capacity and cycle stability.

[0048] Example 6

[0049] A certain mass of purified natural graphite spherical tailings was placed in 30% hydrogen peroxide with a solid-liquid ratio of 1:3, magnetically stirred for 4 hours, rinsed with deionized water, filtered and dried to obtain oxidized graphite. Then it was mixed with a certain mass of citric acid and ammonium chloride aqueous solution, stirred at room temperature for 5 hours, freeze-dried for 24 hours, and pyrolyzed at 800°C for 2 hours under argon atmosphere protection to obtain a carbonized composite material. Polyacrylic acid and an equal molar number of KH550 were mixed evenly and stirred overnight to obtain product 3. The carbonized composite material was added to product 3 and stirred for 12 hours to obtain a mixed solution, and then an excess of glucose reagent was added to the solution, magnetically stirred at 60°C for 6 hours, and the mixed solution was dialyzed and freeze-dried to obtain a hard carbon composite material. The final material was assembled into a semi-button battery for charge and discharge performance testing. Figure 2 It shows that the lithium-ion battery exhibits a specific capacity of 246.33 mA h / g after 1000 cycles at a current density of 1 A / g, and the potassium-ion battery exhibits a specific capacity of 137.64 mA h / g after 250 cycles at a current density of 0.1 A / g. Figure 3 It shows that the specific capacity of lithium-ion batteries before and after adding hard carbon at a current density of 5.0A / g is 25.68mA h / g and 199.82mA h / g respectively, and the specific capacity of potassium-ion batteries before and after adding hard carbon at a current density of 1.0A / g is 9.2mA h / g and 79.3mA h / g respectively. In comparison, it can be clearly seen that after adding hard carbon, better rate performance is obtained under different current densities, and the modified negative electrode material shows higher capacity and cycle stability.

[0050] In summary, the present invention uses natural graphite spherical tailings and hard carbon as important components of the negative electrode material, which are combined with polymer grafting to achieve high-rate long cycle of the battery during charge and discharge, and has excellent cycle stability. The preparation method of the present invention is simple to operate, the required modifiers are all conventional and inexpensive reagents, and the raw materials and synthesis processes are suitable for large-scale production, which makes the prepared negative electrode material and polymer have broad application prospects in lithium-ion batteries.

[0051] The above-mentioned embodiments only express the implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A method for preparing a long-life, low-cost lithium-ion energy storage negative electrode material, characterized in that: The following steps are involved: Step 1, taking a certain mass of purified natural graphite spherical tailings, adding a certain amount of oxidant, stirring at room temperature for 2-8 hours for oxidation treatment, to obtain product 1; Step 2, mixing the product 1 and the hard carbon precursor in a certain proportion, and carbonizing them at a specific temperature, and then keeping them warm for a period of time to obtain the product 2; Step 3, dissolving a plurality of first polymers in a solvent respectively, mixing and stirring at a certain temperature for a period of time to obtain a product 3; Step 4: Mix product 2 and product 3 and stir them for grafting to obtain a mixed solution, then add the second polymer to the mixed solution, stir at 60° C. for 6 hours, dialyze the mixed solution, and dry it to obtain the final product.

2. The method for preparing a long-life, low-cost lithium-ion energy storage negative electrode material according to claim 1, characterized in that: The particle size D50 of the natural graphite spherical tailings in step 1 is 0.5 μm to 10 μm, and the fixed carbon content in the purified natural graphite spherical tailings is greater than 99%.

3. The method for preparing a long-life, low-cost lithium-ion energy storage negative electrode material according to claim 1, characterized in that: In the step 1, the solid-liquid ratio of the natural graphite spherical tailings to the oxidant is 5:1 to 1:50, and the oxidant is one or a combination of two or more of hydrogen peroxide, concentrated nitric acid, concentrated sulfuric acid, concentrated hydrochloric acid, potassium hydroxide, and potassium permanganate.

4. The method for preparing a long-life, low-cost lithium-ion energy storage negative electrode material according to claim 1, characterized in that: The hard carbon precursor is one or a combination of two or more of glucose, biomass tar, phenolic resin, polyvinyl pyrrolidone, citric acid, high-sulfur coal, lignite, and coking coal.

5. The method for preparing a long-life, low-cost lithium-ion energy storage negative electrode material according to claim 1, characterized in that: The mass ratio of the product 1 in step 2 to the hard carbon precursor is 100:5-100:50, the carbonization temperature is 500-1500° C., and the insulation time is 2-6 hours.

6. The method for preparing a long-life, low-cost lithium-ion energy storage negative electrode material according to claim 1, characterized in that: In the step 2, the product 1 and the hard carbon precursor need to be carbonized at high temperature under the protection of a carbonizing atmosphere, wherein the carbonizing atmosphere is any one of an argon atmosphere, a nitrogen atmosphere, and a hydrogen-argon mixed atmosphere, wherein the hydrogen content of the hydrogen-argon mixed atmosphere is 5%.

7. The method for preparing a long-life, low-cost lithium-ion energy storage negative electrode material according to claim 1, characterized in that: The first polymer in step 3 is a combination of two or more of polyacrylic acid, tannic acid, carboxymethyl cellulose, KH550, KH560, phosphoric acid, thermoplastic polyurethane, phytic acid, polyetheramine, tannic acid, polyvinyl alcohol, dopamine, sodium alginate, glutaraldehyde, and chitosan.

8. The method for preparing a long-life, low-cost lithium-ion energy storage negative electrode material according to claim 1, characterized in that: In step 3, the reaction temperature of the multiple first polymers is 30-100° C., and the stirring time is 2-12 hours.

9. The method for preparing a long-life, low-cost lithium-ion energy storage negative electrode material according to claim 1, characterized in that: The second polymer in step 4 is one or a combination of two of β-cyclodextrin, polyvinyl pyrrolidone, water-soluble starch, guar gum, xanthan gum, and glucose.

10. The method for preparing a long-life, low-cost lithium-ion energy storage negative electrode material according to claim 1, characterized in that: In the step 4, the reaction time of mixing and stirring the product 2 and the product 3 to graft the active material is 10-24 hours.

Citation Information

Patent Citations

  • Hard carbon / graphite composite negative electrode material and lithium ion battery as well as preparation method and application thereof

    CN111244407A

  • Method for preparing high-rate lithium battery negative electrode material from natural graphite spherical tailings

    CN114864935A

  • Method for preparing high-rate lithium battery negative electrode material from natural graphite spherical tailings

    CN115799500A

  • Preparation method of special composite binder for silicon-carbon negative electrode

    CN117551417A

  • High-first-efficiency and high-rate silicon-based negative electrode material and preparation method therefor

    WO2022257311A1

Cited By

  • Graded porous hard carbon-silicon composite negative electrode material and preparation method thereof

    CN120565657A