Amorphous lithium hexafluorosilicate, preparation method of amorphous lithium hexafluorosilicate, graphite negative electrode plate, preparation method of graphite negative electrode plate and application of graphite negative electrode plate
By preparing and dispersing amorphized lithium hexafluorosilicate on the surface of the graphite negative electrode sheet under low temperature environment, the ion diffusion kinetics of graphite negative electrode materials in lithium-ion batteries is solved, and the fast charging performance and electrochemical performance are significantly improved.
Patent Information
- Application Number
- CN202411547557.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-01
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-11-01
AI Technical Summary
The graphite anode material of lithium-ion batteries has a slow ion diffusion kinetic process and a cyclic process of lithium dendrites, which limits the fast charging capability.
Reacting silicon, fluorine and lithium sources in a non-aqueous solvent under low temperature environments, amorphous lithium hexafluorosilicate is prepared and dispersed on the surface of graphite negative electrode sheet to improve the transfer rate and electrochemistry of lithium ions performance.
By eliminating grain boundary limitations and increasing lithium ion diffusion pathways, the fast charging and electrochemical performance of graphite negative electrode sheets are significantly improved, and the transmission rate and ion conductivity of lithium ions are improved.
Smart Images

Figure CN119059526A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of energy storage technology, and in particular to an amorphous lithium hexafluorosilicate and a preparation method thereof, a graphite negative electrode sheet and a preparation method and application thereof. Background Art
[0002] At present, the negative electrode of lithium-ion batteries is still mainly made of graphite materials, but graphite materials have problems such as slow ion diffusion kinetics and lithium dendrite growth during the cycle process, which restricts the fast charging ability of lithium-ion batteries. Therefore, it is urgent to improve the fast charging ability of graphite negative electrode sheets through effective methods. Summary of the invention
[0003] Based on this, it is necessary to provide an amorphous lithium hexafluorosilicate and a preparation method thereof, a graphite negative electrode sheet and a preparation method and application thereof to address the above problems. The preparation method can obtain amorphous lithium hexafluorosilicate, which can be used in graphite negative electrode sheets to effectively improve their fast charging capability and electrochemical performance.
[0004] A method for preparing amorphous lithium hexafluorosilicate comprises the following steps: In a protective gas atmosphere, a silicon source, a fluorine source and a lithium source are placed in a non-aqueous solvent to prepare a mixed solution; The mixed solution is placed in a low temperature environment below 0° C. to react, and after the reaction is completed, amorphous lithium hexafluorosilicate is separated to obtain.
[0005] In one embodiment, the temperature of the low temperature environment is -40°C to 0°C.
[0006] In one embodiment, the mixed solution is subjected to ultrasonic treatment when reacting in a low temperature environment below 0°C.
[0007] In one embodiment, the frequency of the ultrasonic treatment is 20 KHz to 120 KHz.
[0008] In one embodiment, the silicon source is selected from at least one of elemental silicon, silicon dioxide, silicic acid, hexafluorosilicic acid, silicon tetrafluoride, silicon tetrachloride, silicate, methylchlorosilane, trichloromethylsilane, trichlorohydrosilane, tetravinylsilane or tetraethyl orthosilicate; And / or, the fluorine source is selected from at least one of lithium fluoride, hydrogen fluoride, hexafluorosilicic acid, lithium hexafluorophosphate, lithium tetrafluoroborate, lithium difluorophosphate, lithium bis(trifluoromethanesulfonyl imide) or lithium bis(fluorosulfonyl imide); And / or, the lithium source is at least one selected from elemental lithium, lithium fluoride, lithium hydroxide, lithium carbonate, lithium hexafluorophosphate, lithium tetrafluoroborate, lithium difluorophosphate, lithium bis(trifluoromethanesulfonyl imide) or lithium bis(fluorosulfonyl imide); And / or, the non-aqueous solvent is selected from at least one of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, propylene carbonate, dimethyl ether, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, tetrahydrofuran, 2-methyltetrahydrofuran, acetonitrile, butyronitrile, benzonitrile, ethanedinitrile or acrylonitrile.
[0009] Amorphous lithium hexafluorosilicate prepared by the method for preparing amorphous lithium hexafluorosilicate.
[0010] A graphite negative electrode sheet comprises a current collector and a graphite material layer attached to the surface of the current collector, wherein amorphous lithium hexafluorosilicate is also attached to the surface of the graphite material layer.
[0011] In one embodiment, the amount of the amorphous lithium hexafluorosilicate used is 2 to 20 times the mass of graphite in the graphite material layer.
[0012] A method for preparing the graphite negative electrode sheet comprises the following steps: Providing a prefabricated graphite negative electrode sheet, the prefabricated graphite negative electrode sheet comprising a current collector and a graphite material layer attached to a surface of the current collector; Amorphous lithium hexafluorosilicate is dispersed in a non-aqueous solvent to obtain a dispersion liquid, the dispersion liquid is placed on the surface of the graphite material layer of the prefabricated graphite negative electrode sheet, and the graphite negative electrode sheet is obtained after drying.
[0013] A lithium ion battery comprises the graphite negative electrode sheet.
[0014] In the preparation method of the present invention, the low temperature environment limits the diffusion rate and reaction kinetics of molecules, atoms or ions, and inhibits the nucleation and growth process of the crystal, thereby realizing the preparation of amorphous lithium hexafluorosilicate. The amorphous lithium hexafluorosilicate is composed of short-range disordered quasi-crystalline domains and structural defects such as vacancies and pores. Among them, the short-range disordered quasi-crystalline domains can greatly reduce the migration energy barrier of lithium ions, and the structural defects such as vacancies and pores can provide more channels for lithium ion transmission and shorten the transmission distance. In addition, the amorphous structure eliminates the grain boundary restriction, so that the ions can be transmitted continuously, which is conducive to accelerating the transmission rate of lithium ions and improving the ionic conductivity of amorphous lithium hexafluorosilicate.
[0015] Therefore, using amorphous lithium hexafluorosilicate on the surface of graphite negative electrode sheets can accelerate the transmission rate of lithium ions by eliminating grain boundary restrictions, increasing lithium ion diffusion pathways, shortening paths, etc., thereby improving the fast charging performance and electrochemical performance of graphite negative electrode sheets. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the technical solutions in the embodiments of the present application or the conventional technology, the drawings required for use in the embodiments or the conventional technology descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0017] Figure 1 The first cycle GCD curve of 0.1C of the graphite negative electrode sheet prepared in Example 5, wherein A is the discharge curve and B is the charge curve; Figure 2 The graph of 200 cycles at 1C of the graphite negative electrode sheet prepared in Example 5 is shown; Figure 3 The first cycle GCD curve of 0.1C of the graphite negative electrode sheet prepared in Comparative Example 2, wherein A is the discharge curve and B is the charge curve; Figure 4 The graph of 200 cycles at 1C of the graphite negative electrode sheet prepared in Comparative Example 2; Figure 5 The first cycle GCD curve of the graphite negative electrode sheet prepared by the blank example at 0.1C, where A is the discharge curve and B is the charge curve; Figure 6 This is a 200 cycle curve of the graphite negative electrode sheet prepared using the blank example at 1C. DETAILED DESCRIPTION
[0018] For ease of understanding of the present invention, the present invention will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. On the contrary, the purpose of providing these embodiments or examples is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0019] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific implementation methods or embodiments, and are not intended to limit the present invention. The optional scope of the term "and / or" used herein includes any one of two or more related listed items, and also includes any and all combinations of related listed items, and the combinations include any two related listed items, any more related listed items, or all related listed items.
[0020] In the present invention, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0021] The method for preparing amorphous lithium hexafluorosilicate provided by the present invention comprises the following steps: S11, placing a silicon source, a fluorine source, and a lithium source in a non-aqueous solvent in a protective gas atmosphere to prepare a mixed solution; S12, placing the mixed solution in a low temperature environment below 0° C. for reaction, and separating to obtain amorphous lithium hexafluorosilicate after the reaction is completed.
[0022] In step S11, the protective gas is selected from at least one of nitrogen or an inert gas, and the inert gas is selected from argon, etc. When the silicon source, fluorine source, and lithium source are placed in a non-aqueous solvent, the lithium source, silicon source, and fluorine source are proportioned according to the molar mass ratio between the reactants.
[0023] The silicon source is selected from at least one of silicon salts or organic silicon sources, and can be specifically selected from elemental silicon (Si), silicon dioxide (SiO2), silicic acid (H2SiO3), hexafluorosilicic acid (H2SiF6), silicon tetrafluoride (SiF4), silicon tetrachloride (SiCl4), silicate, methylchlorosilane (CH3ClSi), trichloromethylsilane (Cl3SiCH3), trichlorohydrosilane (SiHCl3), tetravinylsilane (C8H 12 At least one of tetraethyl orthosilicate (TEOS).
[0024] The fluorine source is selected from at least one of lithium fluoride (LiF), hydrogen fluoride (HF), hexafluorosilicic acid (H2SiF6), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium difluorophosphate (LiPO2F2), lithium bis(trifluoromethanesulfonyl imide) (LiTFSI), and lithium bis(fluorosulfonyl imide) (LiFSI).
[0025] The lithium source is selected from at least one of elemental lithium (Li), lithium fluoride (LiF), lithium hydroxide (LiOH), lithium carbonate (Li2CO3), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium difluorophosphate (LiPO2F2), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), and lithium bis(fluorosulfonyl)imide (LiFSI).
[0026] The non-aqueous solvent is selected from at least one of ester solvents, ether solvents, and nitrile solvents, and can be specifically selected from at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), propylene carbonate (PC), dimethyl ether (DE), ethylene glycol dimethyl ether (DME), diethylene glycol dimethyl ether (DCE), tetraethylene glycol dimethyl ether (TGDE), tetrahydrofuran (THF), 2-methyltetrahydrofuran (2-Me-THF), acetonitrile (ACN), butyronitrile (NBR), benzonitrile (BN), ethanedinitrile (EDN), and acrylonitrile (AN).
[0027] In step S12, when the mixed solution is placed in a low temperature environment below 0°C for reaction, the low temperature environment limits the diffusion rate and reaction kinetics of molecules, atoms or ions, inhibits the nucleation and growth process of the crystal, thereby achieving the preparation of amorphous lithium hexafluorosilicate.
[0028] Furthermore, the temperature of the low-temperature environment is preferably between -40°C and 0°C, including but not limited to -40°C, -35°C, -30°C, -25°C, -20°C, -15°C, -10°C, -5°C or 0°C, which can not only realize the preparation of amorphous lithium hexafluorosilicate, but also reduce the cost of realizing a low-temperature environment.
[0029] Optionally, when the mixed solution is placed in a low temperature environment below 0°C for reaction, ultrasonic treatment is also performed, which can not only make the components in the reaction system evenly dispersed, avoid agglomeration, control the particle size, etc., but also further reduce the reaction rate. Preferably, the frequency of the ultrasonic treatment is 20KHz to 120KHz, including but not limited to 20KHz, 25KHz, 30KHz, 35KHz, 40KHz, 45KHz, 50KHz, 55KHz, 60KHz, 65KHz, 70KHz, 75KHz, 80KHz, 85KHz, 90KHz, 95KHz, 100KHz, 105KHz, 110KHz, 115KHz or 120KHz.
[0030] It is understood that after the reaction is completed, centrifugation and washing can be performed in sequence to remove unreacted substances and self-generated impurities of the reactants, and then drying can be performed to remove residual solvents, thereby separating and obtaining amorphous lithium hexafluorosilicate. Optionally, the drying treatment is preferably a vacuum freeze drying treatment, and the vacuum freeze drying treatment temperature is -40°C to -5°C, and the vacuum degree is 10 - ³Pa to 10 -4 Pa, time is from 10h to 20h.
[0031] The present invention also provides an amorphous lithium hexafluorosilicate prepared by the above-mentioned amorphous lithium hexafluorosilicate preparation method. The amorphous lithium hexafluorosilicate is composed of short-range disordered quasi-crystalline domains and structural defects such as vacancies and pores. The short-range disordered quasi-crystalline domains can greatly reduce the migration energy barrier of lithium ions, and the structural defects such as vacancies and pores can provide more channels for lithium ion transmission and shorten the transmission distance. In addition, the amorphous structure eliminates the grain boundary restrictions, so that ions can be transmitted continuously, which is conducive to accelerating the transmission rate of lithium ions and improving the ionic conductivity of the amorphous lithium hexafluorosilicate.
[0032] The present invention also provides a graphite negative electrode sheet, comprising a current collector and a graphite material layer attached to the surface of the current collector, wherein amorphous lithium hexafluorosilicate is also attached to the surface of the graphite material layer, wherein the graphite material layer is made of graphite, a binder, a conductive agent, etc. in proportion.
[0033] Optionally, the amount of the amorphous lithium hexafluorosilicate used is 2 to 20 times the mass of graphite in the graphite material layer.
[0034] Since the surface of the graphite negative electrode sheet of the present invention has amorphous lithium hexafluorosilicate, the transmission rate of lithium ions can be accelerated by eliminating grain boundary restrictions, increasing lithium ion diffusion pathways, shortening paths, etc. Therefore, the graphite negative electrode sheet of the present invention has better fast charging performance and electrochemical performance.
[0035] The present invention also provides a method for preparing a graphite negative electrode sheet, comprising the following steps: S21, providing a prefabricated graphite negative electrode sheet, wherein the prefabricated graphite negative electrode sheet comprises a current collector and a graphite material layer attached to a surface of the current collector; S22, dispersing amorphous lithium hexafluorosilicate in a non-aqueous solvent to obtain a dispersion, and then placing the dispersion on the surface of the graphite material layer of the prefabricated graphite negative electrode sheet, and obtaining a graphite negative electrode sheet after drying.
[0036] It can be understood that the prefabricated graphite negative electrode sheet in step S21 is a traditional graphite negative electrode sheet, which is prepared by mixing components such as graphite, a conductive agent and a binder to form a slurry, coating the slurry on a current collector, and drying and slicing the slurry. The present invention mainly uses amorphous lithium hexafluorosilicate to treat the traditional graphite negative electrode sheet to improve the fast charging performance and electrochemical properties of the graphite negative electrode sheet.
[0037] Optionally, the non-aqueous solvent described in step S22 is selected from at least one of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, propylene carbonate, dimethyl ether, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, tetrahydrofuran, 2-methyltetrahydrofuran, acetonitrile, butyronitrile, benzonitrile, ethanedinitrile or acrylonitrile, and the dispersion is placed on the surface of the graphite material layer of the prefabricated graphite negative electrode sheet by coating, dripping, etc.
[0038] The present invention also provides a lithium ion battery, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the negative electrode sheet is the graphite negative electrode sheet.
[0039] Since amorphous lithium hexafluorosilicate is used on the surface of the graphite negative electrode sheet used in the lithium ion battery of the present invention, the transmission rate of lithium ions can be accelerated by eliminating grain boundary restrictions, increasing lithium ion diffusion pathways, shortening paths, etc. Therefore, the lithium ion battery of the present invention has better fast charging performance and electrochemical performance.
[0040] Hereinafter, the amorphous lithium hexafluorosilicate and its preparation method, the graphite negative electrode sheet and its preparation method and application will be further described through the following specific examples.
[0041] Example 1 In a glove box under an argon atmosphere, silicon powder, lithium hydroxide and hydrogen fluoride in a molar mass ratio of 1:2:6 were added to an acetonitrile solvent and sealed to obtain a mixed solution, which was then subjected to ultrasonic treatment at 0°C with an ultrasonic frequency of 80 KHz. After the reaction was completed, the crystalline product was separated by a vacuum filtration device, and the crystalline product was washed with an acetonitrile solution, and then vacuum freeze-dried at -35°C with a vacuum degree of 10 -3 Pa, the drying time is 15h, and amorphous lithium hexafluorosilicate is obtained.
[0042] Example 2 In a glove box under an argon atmosphere, silicon dioxide, lithium hydroxide and hydrogen fluoride in a molar mass ratio of 1:2:6 were added to an acetonitrile solvent and sealed to obtain a mixed solution, which was then ultrasonically treated at -4°C with an ultrasonic frequency of 75 kHz. After the reaction was completed, the crystalline product was separated by a vacuum filtration device, and the crystalline product was washed several times with an acetonitrile solution, and then vacuum freeze-dried at -35°C with a vacuum degree of 10 -3 Pa, the drying time is 15h, and amorphous lithium hexafluorosilicate is obtained.
[0043] Example 3 In a glove box under an argon atmosphere, silicon dioxide, lithium hexafluorophosphate and hydrogen fluoride in a molar mass ratio of 1:1:6 were added to a mixed solvent and sealed to obtain a mixed solution, which was then ultrasonically treated at -9°C with an ultrasonic frequency of 70 kHz. After the reaction was completed, the crystalline product was separated by a vacuum filtration device, and the crystalline product was washed several times with an acetonitrile solution, and then vacuum freeze-dried at -35°C with a vacuum degree of 10 -3 Pa, the drying time is 15h, and amorphous lithium hexafluorosilicate is obtained.
[0044] Example 4 In a glove box under an argon atmosphere, silicic acid, lithium fluoride and hydrogen fluoride in a molar mass ratio of 1:6:3 were added to a mixed solvent and sealed to obtain a mixed solution, which was then ultrasonically treated at -14°C with an ultrasonic frequency of 60 kHz. After the reaction was completed, the crystalline product was separated by a vacuum filtration device, and the crystalline product was washed several times with an acetonitrile solution, and then vacuum freeze-dried at -35°C with a vacuum degree of 10 -3 Pa, the drying time is 15h, and amorphous lithium hexafluorosilicate is obtained.
[0045] Example 5 In a glove box under an argon atmosphere, hexafluorosilicic acid and lithium hydroxide in a molar mass ratio of 1:2 were added to a mixed solvent and sealed to obtain a mixed solution, which was then ultrasonically treated at -18°C with an ultrasonic frequency of 50 kHz. After the reaction was completed, the crystalline product was separated by a vacuum filtration device, and the crystalline product was washed several times with an acetonitrile solution, and then vacuum freeze-dried at -35°C with a vacuum degree of 10 -3 Pa, the drying time is 15h, and amorphous lithium hexafluorosilicate is obtained.
[0046] Example 6 In a glove box under an argon atmosphere, hexafluorosilicic acid and lithium carbonate in a molar mass ratio of 1:1 were added to a mixed solvent and sealed to obtain a mixed solution, which was then ultrasonically treated at -22°C with an ultrasonic frequency of 45 kHz. After the reaction was completed, the crystalline product was separated by a vacuum filtration device, and the crystalline product was washed several times with an acetonitrile solution, and then vacuum freeze-dried at -35°C with a vacuum degree of 10 -3 Pa, the drying time is 15h, and amorphous lithium hexafluorosilicate is obtained.
[0047] Example 7 In a glove box under an argon atmosphere, silicon tetrachloride and lithium fluoride in a molar mass ratio of 1:6 were added to a mixed solvent and sealed to obtain a mixed solution, which was then ultrasonically treated at -30°C with an ultrasonic frequency of 40 kHz. After the reaction was completed, the crystalline product was separated by a vacuum filtration device, and the crystalline product was washed several times with an acetonitrile solution, and then vacuum freeze-dried at -35°C with a vacuum degree of 10 -3 Pa, the drying time is 15h, and amorphous lithium hexafluorosilicate is obtained.
[0048] Example 8 In a glove box under an argon atmosphere, tetraethyl orthosilicate, lithium fluoride and hydrogen fluoride in a molar mass ratio of 1:2:6 were added to a mixed solvent and sealed to obtain a mixed solution, which was then ultrasonically treated at -35°C with an ultrasonic frequency of 30 kHz. After the reaction was completed, the crystalline product was separated by a vacuum filtration device, and the crystalline product was washed several times with an acetonitrile solution, and then vacuum freeze-dried at -35°C with a vacuum degree of 10 -3 Pa, the drying time is 15h, and amorphous lithium hexafluorosilicate is obtained.
[0049] Example 9 The only difference between Example 9 and Example 5 is that no ultrasonic treatment is performed during the reaction.
[0050] Comparative Example 1 In a glove box under an argon atmosphere, silicic acid, lithium fluoride and hydrofluoric acid in a molar mass ratio of 1:6:3 were placed in a reaction kettle, and an appropriate amount of acetonitrile was added and mixed evenly, then sealed and kept at 100°C for 5 hours. After cooling, the crystalline product was separated by a vacuum filtration device, and the crystalline product was washed several times with acetonitrile solution, and then vacuum freeze-dried at -35°C with a vacuum degree of 10 -3 Pa, drying time is 15h, and lithium hexafluorosilicate crystals are obtained.
[0051] Comparative Example 2 In a glove box under an argon atmosphere, hexafluorosilicic acid and lithium hydroxide in a molar mass ratio of 1:2 were placed in a reaction kettle, and an appropriate amount of acetonitrile was added and mixed evenly, then sealed and kept at 100°C for 5 hours. After cooling, the crystalline product was separated by a vacuum filtration device, and the crystalline product was washed several times with acetonitrile solution, and then vacuum freeze-dried at -35°C with a vacuum degree of 10 -3 Pa, drying time is 15h, and lithium hexafluorosilicate crystals are obtained.
[0052] Application blank example Weigh 320 mg of artificial graphite material, 40 mg of conductive carbon black and 40 mg of carboxymethyl cellulose, add appropriate amount of deionized water and use planetary ball mill for 2 h, apply the milled slurry on the current collector, and cut it into graphite negative electrode sheets with a diameter of 12 mm after vacuum drying at 80 ° C for 12 h. The loading is 3 mg / cm 2 .
[0053] Then, metallic lithium was used as the counter electrode and reference electrode, PP membrane was selected as the diaphragm, LiPF6 with a concentration of 1 mol / L was used as the electrolyte, and the solvent was a mixed solution of diethyl carbonate and ethylene carbonate with a volume ratio of 1:1. The button battery was assembled in a glove box with an argon atmosphere.
[0054] Application Example 1 to Application Example 9 The difference between Application Examples 1 to 9 and the Blank Example is that the amorphous lithium hexafluorosilicate prepared in Application Examples 1 to 9 is uniformly dispersed in a dimethyl carbonate and ethylene carbonate solvent mixed in a volume ratio of 1:1, and then dropped on the surface of the graphite negative electrode sheet respectively.
[0055] Application Comparative Example 1 to Application Comparative Example 2 The difference between Application Example 1 to Application Example 2 and the Blank Example is that the lithium hexafluorosilicate crystals prepared in Application Example 1 to Application Example 2 are uniformly dispersed in a dimethyl carbonate and ethylene carbonate solvent mixed in a volume ratio of 1:1, and then dropped on the surface of the graphite negative electrode sheet respectively.
[0056] The electrochemical performance test of the button cell obtained above was carried out on the Xinwei battery test system. The charge and discharge voltage range was 0.005V-2V, the current density was 0.1C, 1C=372mA / g, and the test results were as follows: Figures 1 to 6 And as shown in Table 1.
[0057] Table 1 Combination Figures 1 to 6 As shown in Table 1, the amorphous lithium hexafluorosilicate prepared by the present invention shows higher ionic conductivity before and after battery cycling, and at the same time, the 1C large current charge and discharge performance is better. Therefore, the lithium hexafluorosilicate prepared by the present invention can accelerate the ion transmission rate and improve the fast charging performance and electrochemical performance of the graphite negative electrode sheet.
[0058] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0059] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing amorphous lithium hexafluorosilicate, characterized in that: The following steps are involved: In a protective gas atmosphere, a silicon source, a fluorine source and a lithium source are placed in a non-aqueous solvent to prepare a mixed solution; The mixed solution is placed in a low temperature environment below 0° C. to react, and after the reaction is completed, amorphous lithium hexafluorosilicate is separated to obtain.
2. The method for preparing amorphous lithium hexafluorosilicate according to claim 1, characterized in that: The temperature of the low temperature environment is -40°C to 0°C.
3. The method for preparing amorphous lithium hexafluorosilicate according to claim 1, characterized in that: When the mixed solution is placed in a low temperature environment below 0° C. for reaction, ultrasonic treatment is also performed.
4. The method for preparing amorphous lithium hexafluorosilicate according to claim 3, characterized in that: The frequency of the ultrasonic treatment is 20 KHz to 120 KHz.
5. The method for preparing amorphous lithium hexafluorosilicate according to any one of claims 1 to 4, characterized in that: The silicon source is selected from at least one of elemental silicon, silicon dioxide, silicic acid, hexafluorosilicic acid, silicon tetrafluoride, silicon tetrachloride, silicate, methylchlorosilane, trichloromethylsilane, trichlorohydrosilane, tetravinylsilane or tetraethyl orthosilicate; And / or, the fluorine source is selected from at least one of lithium fluoride, hydrogen fluoride, hexafluorosilicic acid, lithium hexafluorophosphate, lithium tetrafluoroborate, lithium difluorophosphate, lithium bis(trifluoromethanesulfonyl imide) or lithium bis(fluorosulfonyl imide); And / or, the lithium source is at least one selected from elemental lithium, lithium fluoride, lithium hydroxide, lithium carbonate, lithium hexafluorophosphate, lithium tetrafluoroborate, lithium difluorophosphate, lithium bis(trifluoromethanesulfonyl imide) or lithium bis(fluorosulfonyl imide); And / or, the non-aqueous solvent is selected from at least one of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, propylene carbonate, dimethyl ether, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, tetrahydrofuran, 2-methyltetrahydrofuran, acetonitrile, butyronitrile, benzonitrile, ethanedinitrile or acrylonitrile.
6. Amorphous lithium hexafluorosilicate prepared by the method for preparing amorphous lithium hexafluorosilicate according to any one of claims 1 to 5.
7. A graphite negative electrode sheet, comprising a current collector and a graphite material layer attached to the surface of the current collector, characterized in that: Amorphous lithium hexafluorosilicate is also attached to the surface of the graphite material layer.
8. The graphite negative electrode sheet according to claim 7, characterized in that: The amount of the amorphous lithium hexafluorosilicate used is 2 to 20 times the mass of the graphite in the graphite material layer.
9. A method for preparing a graphite negative electrode sheet according to claim 7 or claim 8, characterized in that: The following steps are involved: Providing a prefabricated graphite negative electrode sheet, the prefabricated graphite negative electrode sheet comprising a current collector and a graphite material layer attached to a surface of the current collector; Amorphous lithium hexafluorosilicate is dispersed in a non-aqueous solvent to obtain a dispersion liquid, the dispersion liquid is placed on the surface of the graphite material layer of the prefabricated graphite negative electrode sheet, and the graphite negative electrode sheet is obtained after drying.
10. A lithium ion battery, characterized in that: Comprising the graphite negative electrode sheet as claimed in claim 7 or claim 8.
Citation Information
Patent Citations
Method for producing polycrystalline silicon
CN101795964A
Anode active material for lithium storage battery and lithium storage battery having the same
CN101872861A
Method of extracting high-purity fluosilicic acid and silicon dioxide by utilizing industrial fluorine-containing tail gas acid
CN103922345A
Method for producing sodium fluoride from lithium source lithium extraction waste liquid and method for co-producing sodium fluoride and potassium fluosilicate
CN105293529A
Novel positive electrode material manganese lithium fluosilicate and hydrothermal preparation method
CN108417833A