Niobium dioxide as well as preparation method and application thereof

By ball milling of niobium pentachloride and calcium carbide at room temperature, the preparation of niobium dioxide is achieved, solving the problems of inconvenient high-temperature preparation and high energy consumption. It is suitable for potassium and sodium ion battery negative electrode materials and has low energy consumption. and the advantages of simplifying the equipment.

CN119059562APending Publication Date: 2024-12-03SHANGHAI NORMAL UNIVERSITY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411183737.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing preparation methods of niobium dioxide require high-temperature heat treatment, which is inconvenient to operate and high energy consumption, making it difficult to achieve room temperature preparation.

Method used

By ball milling niobium pentachloride and calcium carbide, then washing and vacuum drying, the ball milling of the planetary ball mill was used for room temperature, with a rotation speed of 400-600 rpm, and a time of 0.5-1 hour, niobium pentachloride and calcium carbide The molar ratio is 1:0.8 to 1.2, ethanol and deionized water are used for washing, and dried at 40 to 60°C to achieve the preparation of tetragonal niobium dioxide.

Benefits of technology

No high-temperature heat treatment is required, which significantly reduces energy consumption, simplifies equipment configuration, is gentle in operation, is suitable for energy saving and emission reduction, is suitable for potassium and sodium ion battery negative electrode materials, with the first charging specific capacity of 131mAh g-1 and 101mAh g-1, respectively.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059562A_ABST
    Figure CN119059562A_ABST
Patent Text Reader

Abstract

The invention relates to niobium dioxide as well as a preparation method and application thereof, and the niobium dioxide is directly prepared by taking calcium carbide and niobium pentachloride as raw materials and adopting a normal-temperature mechanical ball milling method. Compared with the prior art, the preparation method has the advantages of no need of high-temperature heat treatment, simplicity, convenience, rapidness, energy conservation and the like, the prepared niobium dioxide can be applied to the negative electrode material of the secondary battery, and the application of the niobium dioxide as the negative electrode material is mainly based on unique physical and chemical properties including high theoretical capacity and good electrochemical stability and thermal stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of advanced materials, and specifically relates to niobium dioxide and a preparation method and application thereof. Background Art

[0002] The room temperature form of niobium dioxide (NbO2) has a short Nb-Nb bond length, a tetragonal superstructure, a rutile sublattice, and a space group of It has broad application prospects in the fields of biosensing, electrocatalysis and energy storage (such as secondary batteries). The metal ions in NbO2 tend to pair along the fourfold

[001] axis and along the shared edge chains, and the Nb-Nb bond lengths alternate. and It is conducive to the sodium / potassium ion intercalation reaction and intralayer diffusion; the ordered pores in the molecular structure can provide additional sodium / potassium storage active sites and promote interlayer migration. Therefore, tetragonal niobium dioxide is a promising negative electrode material for alkali metal ion batteries.

[0003] Patent CN104445403A uses niobium pentoxide as raw material, mixes it with a binder evenly, and presses it into blocks. After granulation, it is loaded into a high-temperature vacuum furnace for sintering and deoxidation to prepare NbO2. Patent CN110021744A uses acrylic resin as a solvent for NbO2 precursor, so that the NbO2 precursor and the resin are evenly mixed and dispersed, and calcined to obtain a nano NbO2 / carbon composite material. Patent CN110963529A mixes reducing metal powder and niobium pentoxide powder and places them in a vacuum atmosphere. After a reduction reaction at 480-520°C for 4-48 hours, it is then treated with acid and dried to obtain a pure phase NbO2 nano powder. The above processes all require high-temperature heat treatment processes, which are inconvenient to operate. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing niobium dioxide at room temperature and its application, wherein the preparation process of niobium dioxide does not require high-temperature heat treatment.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] In one aspect, the present invention provides a method for preparing niobium dioxide, comprising mixing niobium pentachloride and calcium carbide, subjecting the mixture to ball milling, and then washing and drying the mixture to obtain a tetragonal niobium dioxide product.

[0007] Further, the ball milling process is specifically as follows:

[0008] Niobium pentachloride and calcium carbide are placed in a stainless steel ball milling jar containing stainless steel grinding beads, and then placed on a planetary ball mill for ball milling.

[0009] Furthermore, during the ball milling process, the ratio of the total mass of niobium pentachloride and calcium carbide to the mass of the stainless steel ball milling beads is 1:(125-250).

[0010] Furthermore, the ratio of the volume of the stainless steel ball mill to the mass of niobium pentachloride is 250 mL: (1200-2500) mg.

[0011] Furthermore, during the ball milling process, the stainless steel ball milling tank is sealed.

[0012] Furthermore, during the ball milling process, the rotation speed is 400-600 rpm and the time is 0.5-1h.

[0013] Furthermore, the molar ratio of niobium pentachloride to calcium carbide is 1:0.8 to 1:1.2.

[0014] Furthermore, the ball milling process is carried out at room temperature.

[0015] Furthermore, the washing process is specifically as follows: washing with ethanol and deionized water for 3 times.

[0016] Furthermore, the drying process is: vacuum drying at 40-60° C. for 12-24 hours.

[0017] In another aspect, the present invention provides niobium dioxide, which is prepared by any of the preparation methods described above.

[0018] In a third aspect, the present invention also provides a use of niobium dioxide in negative electrode materials for secondary batteries.

[0019] Compared with the prior art, the present invention has the following advantages:

[0020] (1) The reaction at room temperature usually requires less energy, so the energy consumption of the preparation process can be significantly reduced, meeting the requirements of energy conservation and emission reduction.

[0021] (2) Room temperature reactions usually do not require high temperature equipment, such as high temperature furnaces or reactors, which can simplify equipment configuration and reduce equipment investment.

[0022] (3) Room temperature reactions usually have mild operating conditions and are easy to control, reducing the requirements for professional operating skills.

[0023] (4) The first charge capacity of potassium ion battery is 131 mAh g -1 The first charge capacity of sodium-ion batteries is 101 mAh g -1 . BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is the XRD diagram of the product of Example 1 of the present invention.

[0025] Figure 2 The first and second cycle charge-discharge curves of the product of Example 1 of the present invention as the negative electrode material of potassium ion battery, with a charge-discharge current density of 50 mA g -1 , voltage range is 0.005~3.0V(vs.K / K + ).

[0026] Figure 3 The cycle performance curve of the product of Example 1 of the present invention as a negative electrode material for a potassium ion battery, with a charge and discharge current density of 50 mA g -1 , voltage range is 0.005~3.0V(vs.K / K + ).

[0027] Figure 4 This is the XRD diagram of the product of Example 2 of the present invention.

[0028] Figure 5 This is the XRD diagram of the product of Example 3 of the present invention.

[0029] Figure 6 The first and second cycle charge-discharge curves of the product of Example 3 of the present invention as the negative electrode material of sodium ion battery, with a charge-discharge current density of 50 mA g -1 , voltage range is 0.005~3.0V(vs.Na / Na + ).

[0030] Figure 7 This is the XRD diagram of the product of Comparative Example 1 of the present invention.

[0031] Figure 8 This is the XRD diagram of the product of Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0032] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0033] In the following examples, raw materials or processing techniques, unless otherwise specified, are conventional commercially available raw materials or conventional processing techniques in the art.

[0034] Embodiment 1:

[0035] 1620 mg of niobium pentachloride and 385 mg of calcium carbide were weighed into a 250 ml stainless steel ball mill (equipped with 375 g of stainless steel ball mill beads) and sealed; the ball mill was placed in a planetary ball mill, the speed was set to 600 rpm, and ball milling was performed at 25°C for 1 hour; the ball milling product was washed three times with ethanol and deionized water; and vacuum dried at 60°C for 12 hours to obtain niobium dioxide. Figure 1 The X-ray diffraction peaks shown match the characteristic peaks of niobium dioxide (standard card number: 071-0020).

[0036] The niobium dioxide, Super P conductive carbon, and polyvinylidene fluoride binder were weighed in a mass ratio of 8:1:1 and dispersed in 1-methyl-2-pyrrolidone solvent. The slurry was evenly applied on the copper foil, vacuum dried at 90°C for 12 hours, and cut into discs with a diameter of 12 mm as working electrodes. CR2032 button cells were assembled in an argon-filled glove box, in which metallic potassium was used as the counter electrode, 0.8 mol / L KPF6 was dispersed in ethylene carbonate / propylene carbonate (EC / PC, volume ratio of 1:1) solution as the electrolyte, and GF / F glass fiber filter paper was used as the diaphragm. Constant current charge and discharge tests were carried out on the Xinwei battery test system with a current density of 50 mA g -1 , voltage range is 0.005~3.0V(vs.K / K + ). Figure 2 The potential curves of the first and second cycle charge and discharge processes. The first cycle discharge and charge specific capacities are 387 and 131 mAh g, respectively. -1 , corresponding to a coulombic efficiency of 34%. The irreversible capacity comes from the SEI film and irreversible potassium insertion sites generated on the electrode surface. The charge capacity of the second cycle is 117 mAh g -1 , the Coulombic efficiency increased to 82%. Figure 3 50mAg -1 Cyclic performance curve under current density, the reversible capacity after 40 charge and discharge cycles is 75 mAh g -1 , the capacity retention rate relative to the second cycle is 64%.

[0037] Embodiment 2:

[0038] Weigh 2425 mg of niobium pentachloride and 575 mg of calcium carbide into a 250 ml stainless steel ball mill (equipped with 375 g of stainless steel ball mill beads), and seal the ball mill; place the ball mill in a planetary ball mill, set the speed to 400 rpm, and ball mill at 25°C for 1 hour; wash the ball milled product three times with ethanol and deionized water; and vacuum dry it at 40°C for 24 hours to obtain niobium dioxide. Figure 4 The X-ray diffraction peaks shown match the characteristic peaks of tetragonal niobium dioxide (standard card number: 071-0020).

[0039] Embodiment 3:

[0040] 1210 mg of niobium pentachloride and 290 mg of calcium carbide were weighed into a 250 ml stainless steel ball mill (equipped with 375 g of stainless steel ball mill beads) and sealed; the ball mill was placed in a planetary ball mill, the speed was set to 500 rpm, and the ball milling was performed at 25°C for 50 minutes; the ball milling product was washed three times with ethanol and deionized water; and vacuum dried at 50°C for 18 hours to obtain niobium dioxide. Figure 5 The X-ray diffraction peaks shown match the characteristic peaks of tetragonal niobium dioxide (standard card number: 071-0020).

[0041] The niobium dioxide, Super P conductive carbon, and polyvinylidene fluoride binder were weighed in a mass ratio of 6:3:1 and dispersed in 1-methyl-2-pyrrolidone solvent. The slurry was evenly applied on aluminum foil, vacuum dried at 60°C for 16 hours, and cut into discs with a diameter of 12 mm as working electrodes. CR2025 button cells were assembled in an argon-filled glove box, in which metallic sodium was used as the counter electrode, 1 mol / L NaClO4 was dispersed in ethylene carbonate / diethyl carbonate (EC / DEC, volume ratio of 1:1) solution as the electrolyte, and GF / F glass fiber filter paper was used as the diaphragm. Constant current charge and discharge tests were carried out on the Xinwei test system with a current density of 50mAg -1 , voltage range is 0.005~3.0V(vs.Na / Na + ). Figure 6 The potential curves of the first and second cycle charge and discharge processes. The first cycle discharge and charge specific capacities are 436 and 101 mAh g respectively. -1 , corresponding to a coulombic efficiency of 23%. The irreversible capacity comes from the SEI film and irreversible sodium insertion sites generated on the electrode surface. The charge capacity of the second cycle is 100 mAh g -1 , the Coulombic efficiency increased to 76%.

[0042] Comparative Example 1

[0043] Weigh 1620 mg of niobium pentachloride and 385 mg of calcium carbide into a 250 ml stainless steel ball mill (equipped with 375 g of stainless steel ball mill beads), evacuate the ball mill and seal it; place the ball mill in a planetary ball mill, set the speed to 600 rpm, and ball mill at 25°C for 1 hour; wash the ball milled product with ethanol and deionized water three times; and vacuum dry it at 60°C for 12 hours. Figure 7 The X-ray diffraction peak shown does not match the characteristic peak of niobium dioxide (standard card number: 071-0020), and niobium dioxide cannot be directly prepared under this condition.

[0044] Comparative Example 2:

[0045] Weigh 1620 mg of niobium pentachloride and 385 mg of calcium carbide into a 250 ml stainless steel ball mill (equipped with 375 g of stainless steel ball mill beads), replace all the air in the ball mill with oxygen, and seal it; place the ball mill in a planetary ball mill, set the speed to 600 rpm, and ball mill at 25°C for 1 hour; wash the ball milled product with ethanol and deionized water three times; and vacuum dry it at 60°C for 12 hours. Figure 8 The X-ray diffraction spectrum of the product shows that the product is a mixture of niobium dioxide and niobium pentoxide of various crystal forms.

[0046] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A method for preparing niobium dioxide, characterized in that: Niobium pentachloride and calcium carbide are mixed and ball-milled, and then washed and dried to obtain a tetragonal niobium dioxide product.

2. The method for preparing niobium dioxide according to claim 1, characterized in that: The specific process of ball milling is as follows: Niobium pentachloride and calcium carbide are placed in a stainless steel ball milling jar containing stainless steel grinding beads, and then placed on a planetary ball mill for ball milling.

3. The method for preparing niobium dioxide according to claim 2, characterized in that: During the ball milling process, the ratio of the total mass of niobium pentachloride and calcium carbide to the mass of the stainless steel ball milling beads is 1:(125-250).

4. The method for preparing niobium dioxide according to claim 2, characterized in that: During the ball milling process, the rotation speed is 400-600 rpm and the time is 0.5-1h.

5. The method for preparing niobium dioxide according to claim 2, characterized in that: The ratio of the volume of the stainless steel ball mill to the mass of niobium pentachloride is 250 mL: (1200-2500) mg.

6. The method for preparing niobium dioxide according to claim 1, characterized in that: The molar ratio of niobium pentachloride to calcium carbide is 1:0.8 to 1:1.

2.

7. The method for preparing niobium dioxide according to claim 1, characterized in that: The ball milling process is carried out at room temperature and under sealed conditions.

8. The method for preparing niobium dioxide according to claim 1, characterized in that: The specific washing process is as follows: washing with ethanol and deionized water three times; The drying process is: vacuum drying at 40-60°C for 12-24 hours.

9. Niobium dioxide, prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the niobium dioxide as claimed in claim 9 in negative electrode materials for secondary batteries.

Citation Information

Patent Citations

  • Method for preparing niobium oxide and product prepared by method

    CN104445403A

  • Preparation method of nano niobium dioxide / carbon lithium ion battery negative electrode material

    CN110021744A

  • Pure-phase nanopowder of low-valence oxide of niobium, and preparation method and application thereof

    CN110963529A