Method for low-temperature in-situ loading of cerium dioxide by using bacterial cellulose and free radical quenching application thereof

By adsorbing Ce3+ with the surface of bacterial cellulose at room temperature and forming ceria/bacterial cellulose composite materials, the problem of easy agglomeration of ceria nanoparticles in high-temperature preparation is solved, and the preparation of high dispersion and low energy consumption is achieved. Improves its effect in free radical quenching.

CN119059581APending Publication Date: 2024-12-03NANJING UNIV OF SCI & TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410994125.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Ceria nanoparticles are prone to agglomeration during high temperature preparation, resulting in poor dispersion and high energy consumption, limiting their application in industrial wastewater treatment.

Method used

Ce3+ is adsorbed by hydroxyl groups on the surface of bacterial cellulose at room temperature, and C6H12N4 is used as a precipitant to gradually form Ce(OH)4, and ceria/bacterial cellulose composite material loaded on bacterial cellulose is formed by air oxidation to avoid high temperature preparation.

Benefits of technology

The high dispersion and low energy consumption preparation of ceria nanoparticles are achieved, which improves its effect in free radical quenching and is suitable for industrial mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059581A_ABST
    Figure CN119059581A_ABST
Patent Text Reader

Abstract

The invention discloses a method for low-temperature in-situ loading of cerium dioxide by using bacterial cellulose and free radical quenching application thereof. The invention relates to a method for loading cerium dioxide on bacterial cellulose at low temperature in situ, which comprises the following steps: (1) dispersing bacterial cellulose in a solvent at room temperature to obtain a dispersion liquid 1; (2) adding Ce (NO3) 2.6 H2D into the dispersion liquid 1, and mixing to obtain dispersion liquid 2; (3) adding a C6H12N4 solution into the dispersion liquid 2, and stirring to obtain a precursor 1; (4) centrifugally washing the precursor 1 to obtain a precursor 2; and (5) drying the precursor 2 to obtain the cerium dioxide / bacterial cellulose composite material. According to the invention, bacterial cellulose is used as a carrier material, and cerium dioxide nanoparticles which are uniformly distributed on a bacterial cellulose three-dimensional network and are small in size and high in dispersity are obtained under the conditions of room temperature and low energy consumption. A Fenton system test shows that the composite material has a good free radical quenching effect, which shows that the composite material has huge potential application in the aspects of elimination of free radicals in industrial wastewater and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of composite materials, and particularly relates to a method for utilizing bacterial cellulose to load cerium dioxide in situ at low temperature and a free radical quenching application thereof. Background Art

[0002] Free radical quenching is an important process in industrial wastewater treatment. Free radicals are highly reactive molecules or atoms with unpaired electrons that play a key role in chemical reactions. In industrial wastewater treatment, free radical quenching refers to the process of neutralizing or eliminating free radicals by adding appropriate side-reacting agents. This is usually achieved by adding a substance called an antioxidant. Antioxidants are able to capture free radicals and stabilize them, thereby preventing them from continuing to participate in harmful chemical reactions.

[0003] Cerium dioxide (CeO2) is a transition metal oxide material with its reversible Ce 3+ With Ce 4+ The conversion between and the crystal structure with oxygen vacancies have attracted extensive attention. In particular, cerium dioxide nanoparticles (CeO2-NPs) have been widely used in the fields of free radical quenching and biological antioxidant. However, cerium dioxide nanoparticles agglomerate during high-temperature preparation and application, resulting in a significant decrease in their specific surface area, which limits their further development and application. Many studies have shown that preparing them as supported cerium dioxide nanoparticle materials can effectively improve the dispersion stability and specific surface area of ​​the particles.

[0004] Bacterial cellulose (BC) is produced by bacteria such as Acetobacterium, and has the advantages of bioaffinity, biodegradability, renewability, high mechanical and chemical stability, and high specific surface area given by porous structure. It can be used as an excellent carrier for many nanomaterials. In addition, there are a large number of hydroxyl groups on the surface of bacterial cellulose, which are suitable for acting as templates and end-capping agents for metal or metal oxide particles to prepare multifunctional bacterial cellulose hybrid multifunctional materials. Summary of the invention

[0005] The problem to be solved by the present invention is that the present invention aims to solve the problems of poor dispersibility, easy agglomeration and high energy consumption of high-temperature preparation of cerium dioxide. 3+ Adsorption of C6H 12 N4 is used as a precipitant and is oxidized by air to stably load Ce(OH)4 on bacterial cellulose, which is then dried to obtain a cerium dioxide / bacterial cellulose composite material, solving the problems of poor dispersibility, easy agglomeration, and high energy consumption of high-temperature preparation of cerium dioxide materials.

[0006] The technical solution adopted to solve the technical problem is to provide a method for low-temperature in-situ loading of cerium dioxide on bacterial cellulose, comprising the following steps:

[0007] Step 1: Ultrasonic dispersion of bacterial cellulose whiskers in deionized water at room temperature to obtain dispersion 1;

[0008] Step 2: Add Ce(NO3)2·6H2O to dispersion 1 and mix thoroughly to obtain dispersion 2;

[0009] Step 3: Add C6H2O dropwise to dispersion 2 12 N4 solution and stirred for 6-24h to obtain precursor 1;

[0010] Step 4: centrifuge and wash the precursor 1 to obtain the precursor 2;

[0011] Step 5: Precursor 2 is dried at 80° C. for 24 hours to obtain a cerium dioxide / bacterial cellulose composite material.

[0012] Step 6: Conduct free radical quenching rate test on the cerium dioxide / bacterial cellulose composite material.

[0013] The beneficial effects of the technical solution of the present invention are as follows: bacterial cellulose is used as a nanoparticle carrier, Ce(NO3)2·6H2O is used as a cerium source, and C6H 12 N4 acts as a precipitant, and the hydroxyl groups on the surface of bacterial cellulose adsorb cerium metal cations through electrostatic adsorption. 12 N4 first acts as a ligand to stabilize the cerium metal cations in the system, and also acts as a precipitant to slowly decompose and form an alkaline microenvironment to precipitate the cerium metal cations. 3+ It is transformed into Ce(OH)4 loaded on bacterial cellulose, and finally dried to form cerium dioxide / fine cation adsorption, C6H 12 N4 first acts as a ligand to stabilize the cerium metal cations in the system, and also acts as a precipitant to slowly decompose and form an alkaline microenvironment to precipitate the cerium metal cations. 3+ It is transformed into Ce(OH)4 loaded on bacterial cellulose and finally dried to form a cerium dioxide / bacterial cellulose composite material.

[0014] Preferably, in step 1, the mass ratio of bacterial cellulose whiskers to water is 1:16; and the solvent is deionized water.

[0015] Preferably, the mass ratio of Ce(NO3)2·6H2O to bacterial cellulose added in step 2 is (1-8):25.

[0016] Preferably, step 3C6H 12The volume ratio of N4 solution to dispersion 2 is 1:1, and the solvent is deionized water.

[0017] Preferably, step 4C6H 12 C6H in N4 solution 12 Mass ratio of N4 to water (1-6): 80.

[0018] Preferably, in step 5, the centrifugal speed is 6000-8200 rpm, and the centrifugal time is 5 min; and the washing is 3 times of deionized water washing.

[0019] Preferably, in step 5, the drying temperature is 80° C. and the drying time is 24 h.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] (1) Using bacterial cellulose as a carrier material, adjust the Ce(NO3)2·6H2O and C6H 12 The addition amount of N4 was reduced, and a cerium dioxide / bacterial cellulose composite material loaded with highly dispersed cerium dioxide nanoparticles was successfully obtained; (2) Low-temperature synthesis avoided the high energy consumption required for high-temperature synthesis, and the operation was simple and easy to achieve industrial large-scale preparation; (3) The prepared cerium dioxide / bacterial cellulose composite material had a good free radical quenching effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 is the XPS spectrum of the cerium dioxide / bacterial cellulose composite material synthesized in Example 1;

[0023] Figure 2 is the XRD pattern of the cerium dioxide / bacterial cellulose composite material synthesized in Example 1;

[0024] Figure 3 is a SEM image (a) of the cerium dioxide / bacterial cellulose composite material synthesized in Example 1 and the corresponding EDS image and element content image of C, O and Ce elements;

[0025] Figure 4 This is a diagram showing the free radical quenching effect of the cerium dioxide / bacterial cellulose composite material synthesized in Example 1. DETAILED DESCRIPTION

[0026] The present invention is further described in detail below in conjunction with embodiments and drawings.

[0027] Example 1

[0028] A method for in-situ loading of cerium dioxide on bacterial cellulose at low temperature comprises the following steps:

[0029] Step 1: At room temperature, 5 g of bacterial cellulose whiskers were added to 80 g of deionized water, and ultrasonically dispersed for 1 h to obtain a uniformly dispersed bacterial cellulose whisker dispersion 1;

[0030] Step 2: Add 0.4 g Ce(NO3)2·6H2O to dispersion 1 and continue stirring for 6 h to fully absorb Ce. 3+ , get Ce 3+ uniformly mixed bacterial cellulose whisker dispersion 2;

[0031] Step 3: 3g C6H 12 N4 was added to 80 g of deionized water and stirred for 0.5 h to make C6H 12 N4 is fully dissolved to obtain C6H 12 N4 aqueous solution. During continuous stirring, an equal volume of C6H 12 The N4 aqueous solution was added dropwise into the dispersion 2 and stirred for 12 h to obtain the precursor 1:

[0032] Step 4: Centrifuge the precursor 1 at 6000 rpm for 5 min, repeat the centrifugation and wash for 3 times, and collect

[0033] Example 2

[0034] A method for in-situ loading of cerium dioxide on bacterial cellulose at low temperature comprises the following steps:

[0035] Step 1: At room temperature, 5 g of bacterial cellulose whiskers were added to 80 g of deionized water, and ultrasonically dispersed for 1 h to obtain a uniformly dispersed bacterial cellulose whisker dispersion 1;

[0036] Step 2: Add 0.4 g Ce(NO3)2·6H2O to dispersion 1 and continue stirring for 6 h to fully absorb Ce. 3+ , get Ce 3 + uniformly mixed bacterial cellulose whisker dispersion 2;

[0037] Step 3: Add 6g C6H 12 N4 was added to 80 g of deionized water and stirred for 0.5 h to make C6H 12 N4 is fully dissolved to obtain C6H 12 N4 aqueous solution. During continuous stirring, an equal volume of C6H 12 The N4 aqueous solution was added dropwise to the dispersion 2 and stirred for 6 h to obtain the precursor 1;

[0038] Step 4: Precursor 1 was centrifuged at 7000 rpm for 5 min, and the obtained precipitate was repeatedly centrifuged and washed 3 times, and the white precipitate after sufficient washing was collected to obtain precursor 2;

[0039] Step 5: Transfer the precursor 2 to a culture dish and dry it at 80° C. for 24 h to obtain a light yellow solid, i.e., a cerium dioxide / bacterial cellulose composite material.

[0040] Step 6: Conduct free radical quenching rate test on the cerium dioxide / bacterial cellulose composite material.

[0041] Example 3

[0042] A method for in-situ loading of cerium dioxide on bacterial cellulose at low temperature comprises the following steps:

[0043] Step 1: At room temperature, 5 g of bacterial cellulose whiskers were added to 80 g of deionized water, and ultrasonically dispersed for 1 h to obtain a uniformly dispersed bacterial cellulose whisker dispersion 1;

[0044] Step 2: Add 0.4 g Ce(NO3)2·6H2O to dispersion 1 and continue stirring for 6 h to fully absorb Ce. 3+ , get Ce 3+ uniformly mixed bacterial cellulose whisker dispersion 2;

[0045] Step 3: 1g C6H 12 N4 was added to 80 g of deionized water and stirred for 0.5 h to make C6H 12 N4 is fully dissolved to obtain C6H 12 N4 aqueous solution. While stirring continuously, add an equal volume of C6H 12 The N4 aqueous solution was added dropwise into the dispersion 2 and stirred for 18 h to obtain the precursor 1;

[0046] Step 4: Precursor 1 was centrifuged at 8000 rpm for 5 min, and the obtained precipitate was repeatedly centrifuged and washed 3 times, and the white precipitate after sufficient washing was collected to obtain precursor 2;

[0047] Step 5: Transfer the precursor 2 to a culture dish and dry it at 80° C. for 24 h to obtain a light yellow solid, i.e., a cerium dioxide / bacterial cellulose composite material.

[0048] Step 6: Test the free radical quenching rate of the cerium dioxide bacterial cellulose composite material.

[0049] Example 4

[0050] A method for in-situ loading of cerium dioxide on bacterial cellulose at low temperature comprises the following steps:

[0051] Step 1: At room temperature, 5 g of bacterial cellulose whiskers were added to 80 g of deionized water and ultrasonically dispersed for 1 h to obtain a uniformly dispersed bacterial cerium / bacterial cellulose composite material.

[0052] Step 6: Conduct free radical quenching rate test on the cerium dioxide / bacterial cellulose composite material.

[0053] Example 4

[0054] A method for in-situ loading of cerium dioxide on bacterial cellulose at low temperature comprises the following steps:

[0055] Step 1: At room temperature, 5 g of bacterial cellulose whiskers were added to 80 g of deionized water, and ultrasonically dispersed for 1 h to obtain a uniformly dispersed bacterial cellulose whisker dispersion 1;

[0056] Step 2: Add 0.8 g Ce(NO3)2·6H2O to dispersion 1 and continue stirring for 6 h to fully absorb Ce. 3+ , get Ce 3+ uniformly mixed bacterial cellulose whisker dispersion 2;

[0057] Step 3: 3g C6H 12 N4 was added to 80 g of deionized water and stirred for 0.5 h to make C6H 12 N4 is fully dissolved to obtain C6H 12 N4 aqueous solution. During continuous stirring, an equal volume of C6H 12 The N4 aqueous solution was added dropwise into the dispersion 2 and stirred for 12 h to obtain the precursor 1:

[0058] Step 4: Precursor 1 was centrifuged at 6000 rpm for 5 min, and the obtained precipitate was repeatedly centrifuged and washed 3 times, and the white precipitate after sufficient washing was collected to obtain precursor 2;

[0059] Step 5: Transfer the precursor 2 to a petri dish and dry it at 80 °C for 24 h to obtain a light yellow solid, i.e., the cerium dioxide / bacterial cellulose composite material.

[0060] Step 6: Conduct free radical quenching rate test on the cerium dioxide / bacterial cellulose composite material.

[0061] Comparative Example 1

[0062] A method for in-situ loading of cerium dioxide on bacterial cellulose at low temperature comprises the following steps:

[0063] Step 1: At room temperature, add 5 g of bacterial cellulose whiskers into 80 g of deionized water and disperse them ultrasonically for 1 h to obtain uniformly dispersed bacterial cellulose whiskers. Dispersion temperature 1;

[0064] Step 2: Add 0.2g Ce(NO3)2-6H2O to dispersion 1 and continue stirring for 6h to fully absorb Ce. 3+ , get Ce 3 +uniformly mixed bacterial cellulose whisker dispersion 2;

[0065] Step 3: 1gC6H 12 N4 was added to 80 g of deionized water and stirred for 0.5 h to make C6H 12 N4 is fully dissolved to obtain C6H 12 N4 aqueous solution. During continuous stirring, an equal volume of C6H 12 The N4 aqueous solution was added dropwise into the dispersion 2 and stirred for 24 h to obtain the precursor 1;

[0066] Step 4: Precursor 1 was centrifuged at 7000 rpm for 5 min, and the obtained precipitate was repeatedly centrifuged and washed 3 times, and the white precipitate after sufficient washing was collected to obtain precursor 2;

[0067] Step 5: Transfer the precursor 2 to a culture dish and dry it at 80° C. for 24 h to obtain a light yellow solid, i.e., a cerium dioxide / bacterial cellulose composite material.

[0068] Step 6: Conduct free radical quenching rate test on the cerium dioxide / bacterial cellulose composite material.

[0069] Step 3: Add 6g C6H 12 N4 was added to 80 g of deionized water and stirred for 0.5 h to make C6H 12 N4 is fully dissolved to obtain C6H 12 N4 aqueous solution. During continuous stirring, an equal volume of C6H 12 The N4 aqueous solution was added dropwise into the dispersion 2 and stirred for 12 h to obtain the precursor 1;

[0070] Step 4: Precursor 1 was centrifuged at 5000 rpm for 5 min, and the obtained precipitate was repeatedly centrifuged and washed 3 times, and the white precipitate after sufficient washing was collected to obtain precursor 2;

[0071] Step 5: Transfer the precursor 2 to a culture dish and dry it at 80° C. for 24 h to obtain a light yellow solid, i.e., a cerium dioxide / bacterial cellulose composite material.

[0072] Step 6: Conduct free radical quenching rate test on the cerium dioxide / bacterial cellulose composite material.

Claims

1. A method for in-situ loading of cerium dioxide using bacterial cellulose at low temperature and its free radical quenching application, It is characterized in that The following steps are involved: Step 1: Ultrasonic dispersion of bacterial cellulose whiskers in deionized water at room temperature to obtain dispersion 1: Step 2: Add Ce(NO 3 ) 2 6H 2 O and mix thoroughly to obtain dispersion 2: Step 3: Add C dropwise to dispersion 2 6 H 12 N 4 The solution was stirred for 6-24 hours to obtain precursor 1: Step 4: centrifuge and wash the precursor 1 to obtain the precursor 2; Step 5: Precursor 2 is dried for 24 hours to obtain a cerium dioxide / bacterial cellulose composite material. Step 6: Conduct free radical quenching rate test on the cerium dioxide / bacterial cellulose composite material.

2. A method for in-situ loading of cerium dioxide using bacterial cellulose at low temperature and its free radical quenching application as claimed in claim 1, Features: In the step 1, the mass ratio of bacterial cellulose whiskers to water is 1:16; and the solvent is deionized water.

3. A method for in-situ loading of cerium dioxide using bacterial cellulose at low temperature and its free radical quenching application as claimed in claim 1, Features: In step 2, Ce(NO 3 ) 2 6H 2 The mass ratio of O to bacterial cellulose is (1-8):

25.

4. A method for in-situ loading of cerium dioxide using bacterial cellulose at low temperature and its free radical quenching application as claimed in claim 1, Features: In step 3, C 6 H 12 N 4 The volume ratio of the solution to the dispersion 1 is 1:1, and the solvent is deionized water.

5. A method for in-situ loading of cerium dioxide using bacterial cellulose at low temperature and its free radical quenching application as claimed in claim 1, Features: In step 3, C 6 H 12 N 4 C in solution 6 H 12 N 4 Mass ratio to water (1-6):

80.

6. A method for in-situ loading of cerium dioxide using bacterial cellulose at low temperature and its free radical quenching application as claimed in claim 1, Features: In the step 4, the centrifugal speed is 6000-8000 rpm, and the centrifugal time is 5 min; the washing is performed 3 times with deionized water.

7. A method for in-situ loading of cerium dioxide using bacterial cellulose at low temperature and its free radical quenching application as claimed in claim 1, Features: In step 5, the drying temperature is 80° C. and the drying time is 24 hours.

8. A method for in-situ loading of cerium dioxide using bacterial cellulose at low temperature and its free radical quenching application as claimed in claim 1, Features: In step 6, a Fenton system is used to generate free radicals, wherein the concentrations of ferrous sulfate and hydrogen peroxide are 0.6 mM and 1.0 mM, respectively; the cerium dioxide / bacterial cellulose composite material is introduced into the Fenton system, rhodamine B is used as a color developer, and the concentration of rhodamine B is quantitatively analyzed by ultraviolet-visible spectroscopy to detect the concentration of free radicals.

Citation Information

Patent Citations