High-hardness high-crystallinity transparent glass ceramic and preparation method thereof

Through two-step crystallization process and electric field treatment, combined with appropriate amount of nucleating agent and raw material formula adjustment, the problem of reduced transparency of spinel-based glass ceramics at high temperatures is solved, and transparent glass ceramics with high hardness and high crystallinity are achieved. Excellent optical and mechanical properties.

CN119059737AActive Publication Date: 2024-12-03XUZHOU NORMAL UNIVERSITY +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411209823.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-03
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

The transparency of existing spinel-based glass ceramics is reduced at high temperatures, and transparent glass ceramics with high crystallinity cannot be obtained, and the hardness has not been effectively improved.

Method used

Using a two-step crystallization process, by adding an appropriate amount of nucleating agent to the glass melt and applying an electric field, the crystallization temperature and time are controlled to form uniform small grains, improving grain connection and optical performance, and adjusting the raw material formula and sintering process. Increase the viscosity of residual glass to increase hardness.

Benefits of technology

It has achieved high hardness and high crystallinity production of transparent glass ceramics, with a transmittance of ≥86.5%, and a Vickers hardness of 9.1GPa or above. The process is simple and efficient, and is suitable for large-size preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059737A_ABST
    Figure CN119059737A_ABST
Patent Text Reader

Abstract

The invention discloses a high-hardness high-crystallinity transparent glass ceramic and a preparation method thereof. Weighing a glass powder raw material, grinding the glass powder raw material, adding the ground glass powder raw material into a platinum-rhodium crucible, and melting to obtain molten glass; wherein the glass powder raw material is prepared from the following components in percentage by mass: 0 to 12 weight percent of ZnO, 6 to 18 weight percent of MgO, 22 to 35 weight percent of Al2O3, 40 to 50 weight percent of SiO2, 1 to 3 weight percent of Sb2O3 and 0.5 to 9 weight percent of nucleating agent; pouring the molten glass into a preheated copper mold to obtain a transparent glass block; annealing, cutting and polishing to obtain precursor glass with the thickness of 2mm; and placing the precursor glass between electrode plates, preserving heat for 1-10 hours at the nucleation temperature of 700-900 DEG C, and then preserving heat for 2-8 hours at the crystallization temperature of 900-1150 DEG C to prepare the transparent glass ceramic. Controllable crystallization is achieved by controlling crystallization time and temperature, the crystallinity of the glass ceramic is larger than or equal to 85%, the glass ceramic has good optical quality and transmittance, and the transmittance of the glass ceramic with the thickness of 1.5 mm at the position of 800 nm is larger than or equal to 86.5%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of glass ceramic preparation, and in particular to a transparent glass ceramic with high hardness and high crystallinity and a preparation method thereof. Background Art

[0002] As an important material, glass ceramics have the advantages of excellent mechanical properties, high heat resistance, excellent chemical stability, good optical properties, and flexible design. Among them, spinel glass ceramics are a type of material with excellent optical and mechanical properties, and have broad application prospects in flat panel displays, photovoltaic substrates, high-temperature optical windows, lasers, medical and other fields. Glass ceramics have uneven crystal sizes, large differences in refractive index, and crystal morphology, which will affect the transmittance of microcrystalline glass. Therefore, the raw material formula and proportion are adjusted, the sintering process and system are improved, and appropriate dopants are used to promote balanced grain size and uniform grain distribution, thereby improving the transparency and mechanical properties of glass ceramics.

[0003] At present, there are a large number of literatures on the research of glass ceramics of the spinel system in order to achieve the luminescence regulation of fluorescent ceramics. The literature (ZnO-Al2O3-SiO2 glass ceramics: Influence of composition on crystal phases, crystallite size and appearance, 2021, 120481) shows that the grain size reaches the nanometer level. However, other phases such as Zn2SiO4 and Zn2Ti3O8 will appear, and the refractive index difference between the crystal phases is large, resulting in the opacity of the prepared glass ceramics, and the hardness of the glass ceramics has not been explored. The literature (Crystallization behavior and properties of ZnO-MgO-Al2O3-SiO2 transparent glass-ceramics with SnO2 and ZrO2 as nucleating agents, 2024, 23150-23056) used ZrO2 and SnO2 as nucleating agents to prepare transparent ZnO-MgO-Al2O3-SiO2 (ZMAS) glass-ceramics by melting and two-step heat treatment. SnO2 promoted the formation of ZrO2 nanocrystals and provided nucleation sites for subsequent crystallization. The Vickers hardness was 8.28MPa. However, with the increase of crystallization temperature, the transparency of glass-ceramics decreases, and transparent glass-ceramics with high crystallinity cannot be obtained. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing transparent glass ceramics with high hardness and high crystallinity.

[0005] To achieve the above object, the technical solution adopted by the present invention is as follows: A method for preparing a transparent glass ceramic with high hardness and high crystallinity comprises the following steps:

[0006] (1) weighing a glass powder raw material, grinding the glass powder for 0.5 to 2 hours, adding the glass powder into a platinum-rhodium crucible, and melting the glass powder at 1500 to 1750° C. for 2 to 4 hours to obtain a glass liquid; wherein the glass powder raw material is composed of the following components in weight percentage: ZnO 0 to 12 wt%, MgO 6 to 18 wt%, Al2O3 22 to 35 wt%, SiO2 40 to 50 wt%, Sb2O3 1 to 3 wt%, and a nucleating agent 0.5 to 9 wt%;

[0007] (2) pouring the glass liquid into a preheated copper mold to obtain a transparent glass block;

[0008] (3) annealing the glass block to obtain a precursor glass, and cutting and polishing the precursor glass, wherein the glass thickness is 2 mm;

[0009] (4) The precursor glass is placed between the electrode sheets, first kept at a nucleation temperature of 700 to 900°C for 1 to 10 hours, then kept at a crystallization temperature of 900 to 1150°C for 2 to 8 hours, and then taken out after cooling to room temperature to prepare a transparent glass ceramic.

[0010] Preferably, in step (1), the heating rate of the lifting furnace is 5 to 20° C. / min.

[0011] Preferably, the nucleating agent in step (1) is selected from one or more of P2O5, ZrO2, TiO2, Eu2O3, and CeO2.

[0012] Preferably, in step (2), the preheating temperature of the copper mold is 300-600°C.

[0013] Preferably, in step (4), the glass is annealed in air at 500-800° C. for 4-10 hours.

[0014] Preferably, in step (4), the glass is placed between the positive and negative electrodes of the electrode sheet, the electric field strength is 300 to 1000 V / cm, and when the temperature in the furnace rises to the crystallization temperature, the power is turned on and maintained at the target electric field strength until the crystallization time ends.

[0015] Preferably, step (4) further comprises milling and polishing the crystallized glass ceramics, and the thickness of the glass ceramics is 1.5 mm.

[0016] The residual glass in glass ceramics can play a role in connecting the crystal grains. Reasonable control of the residual glass content can improve the hardness of glass ceramics. At the same time, during the crystallization process, as the crystallization rate increases, the content of alkaline earth metal ions in the residual glass decreases, thereby increasing the viscosity of the residual glass, improving the connection between the crystal grains, and improving the hardness of the glass ceramics. The addition of an appropriate amount of nucleating agent is conducive to the uniform formation of crystal nuclei, thereby improving the uniformity of the crystal grains. During the glass crystallization process, applying an electric field at both ends of the glass is conducive to refining the crystal grains, thereby improving the transmittance of the glass ceramics.

[0017] On the other hand, the present invention also provides a transparent glass ceramic with high hardness and high crystallinity prepared by the above preparation method. The glass ceramic mainly comprises zinc-aluminum spinel and magnesium-aluminum spinel, and a residual glass phase that plays a connecting role.

[0018] The glass ceramic has a particle size of 20 to 100 nm, and the crystal phases form a dense structure. The addition of a nucleating agent can effectively reduce the melting temperature and crystallization temperature of the glass, facilitate the formation of the crystal phase, and improve the stability of the glass. It is transparent in the visible light range, and the transmittance of 1.5 mm thick glass ceramic at a wavelength of 800 nm is ≥86.5%. The nucleating agent provides additional nucleation points, making it easier to form crystal nuclei during the cooling process of the glass melt, and can also control the grain size and distribution in the final glass ceramic.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] (1) The transparent glass ceramics prepared by the present invention achieve controllable crystallization by controlling the crystallization time and temperature through a two-step crystallization method. The nucleating agent provides additional nucleation points, and the grain size and uniformity can be controlled by regulating the crystallization conditions, thereby enhancing the mechanical properties of the material. The crystallinity of the glass ceramics is ≥85%;

[0021] (2) During the crystallization process of the glass provided by the present invention, an electric field is applied to the glass, which is conducive to the formation of the spinel phase, and the generated grains are small and uniform, so the glass ceramic has good optical quality and transmittance. The transmittance of the glass ceramic with a thickness of 1.5 mm at 800 nm is ≥ 86.5%. The residual Zn in the glass phase 2+ ,Mg 2+ The residual glass viscosity increases, which is beneficial to the improvement of the mechanical properties of glass ceramics;

[0022] (3) Based on mature glass forming technology, transparent glass ceramics can be obtained after heat treatment of the precursor glass. The process is simple, efficient, and has high crystallinity. This method can also be used to prepare large-sized transparent glass ceramics. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1The transmittance graphs of the transparent glass ceramics prepared in Examples 1 to 4 of the present invention;

[0024] Figure 2 This is a SEM image of the transparent glass ceramic prepared in Example 1 after being etched by hydrofluoric acid;

[0025] Figure 3 XRD pattern of the transparent glass-ceramic prepared in Example 1;

[0026] Figure 4 This is a Vickers hardness diagram of the transparent glass-ceramics prepared in Examples 1 to 4. DETAILED DESCRIPTION

[0027] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0028] The raw material powders used in the following examples are all commercially available products with a purity greater than 99.9%.

[0029] Example 1

[0030] (1) Weighing glass powder raw materials The following raw materials were weighed according to the following mass percentages: ZnO 10wt%, MgO 15wt%, Al2O3 25wt%, SiO2 45wt%, Sb2O3 1wt%, nucleating agent P2O5 2wt%, and nucleating agent Eu2O3 2wt%. The glass powder was ground for 1.5h and mixed evenly. The mixture was added to a platinum-rhodium crucible, placed in a lifting furnace, heated at a rate of 10°C / min, and melted at 1650°C for 2h to obtain glass liquid.

[0031] (2) pouring the glass liquid into a copper mold preheated to 450°C to form a transparent glass block;

[0032] (3) annealing the glass block at 700° C. for 4 h to obtain a precursor glass, and cutting and polishing the precursor glass to a glass thickness of 2 mm;

[0033] (4) The precursor glass was placed between the electrodes with an electric field strength of 400 V / cm. It was first kept at a nucleation temperature of 780°C for 4 h and then kept at a crystallization temperature of 980°C for 1.5 h. After cooling to room temperature, it was taken out and the surface of the glass ceramic was milled and polished to a thickness of 1.5 mm to obtain a transparent glass ceramic with a crystallization rate of 86%.

[0034] Figure 1The transmittance curve of the transparent glass ceramic prepared in this embodiment is 86.5% at 800nm. The glass ceramic has a high transmittance. The sample without nucleating agent has uneven grain size, which will cause abnormal growth of grains during the crystallization process, resulting in a low transmittance of 67.4%. Since there is no nucleating agent to provide additional nucleation points, the glass crystallization rate is low, at 72.4%.

[0035] Figure 2 This is a SEM image of the transparent glass ceramic prepared in this embodiment after being etched by hydrofluoric acid. The grain size is uniform and the grain size is 20-40 nm.

[0036] Figure 3 The XRD diagram of the transparent glass-ceramic prepared in this example shows that the main crystalline phases generated are magnesium-aluminum spinel and zinc-aluminum spinel, and there is also a residual glass phase that plays a connecting role.

[0037] Figure 4 The Vickers hardness of the transparent glass-ceramic prepared in this embodiment reaches 9.1 GPa.

[0038] Example 2

[0039] (1) Weighing glass powder raw materials The following raw materials were weighed according to the following mass percentages: ZnO 8wt%, MgO 16wt%, Al2O3 30wt%, SiO2 40wt%, Sb2O3 1wt%, and nucleating agent TiO2 5wt%. The glass powder was ground for 2 h to mix evenly, added to a platinum-rhodium crucible, placed in a lifting furnace, heated at a rate of 5°C / min, and melted at 1600°C for 3 h to obtain glass liquid;

[0040] (2) pouring the glass liquid into a copper mold preheated to 500°C to form a transparent glass block;

[0041] (3) annealing the glass block at 750° C. for 6 h to obtain a precursor glass, and cutting and polishing the precursor glass to a glass thickness of 2 mm;

[0042] (4) The precursor glass was placed between the electrodes with an electric field strength of 600 V / cm. It was first kept at a nucleation temperature of 790°C for 6 hours and then kept at a crystallization temperature of 950°C for 2 hours. After cooling to room temperature, it was taken out and the surface of the glass ceramic was milled and polished to a thickness of 1.5 mm to obtain a transparent glass ceramic with a crystallization rate of 88%.

[0043] The transmittance curve and SEM of the transparent glass-ceramic prepared in this embodiment are similar to those in Embodiment 1, the grain size is 25-45 nm, and the Vickers hardness reaches 11.0 GPa.

[0044] Example 3

[0045] (1) Weighing glass powder raw materials The following raw materials were weighed according to the following mass percentages: ZnO 12wt%, MgO 12wt%, Al2O3 26wt%, SiO2 42wt%, Sb2O3 2wt%, nucleating agent TiO2 2wt%, nucleating agent ZrO2 2wt%, nucleating agent Eu2O3 1wt%, nucleating agent CeO2 1wt%, the glass powder was ground for 3h and mixed evenly, added to a platinum-rhodium crucible, placed in a lifting furnace, heated at a rate of 15°C / min, and melted at 1680°C for 2h to obtain glass liquid;

[0046] (2) pouring the glass liquid into a copper mold preheated to 550°C to form a transparent glass block;

[0047] (3) annealing the glass block at 780° C. for 5 h to obtain a precursor glass, and cutting and polishing the precursor glass to a glass thickness of 2 mm;

[0048] (4) The precursor glass is placed between the electrode sheets with an electric field strength of 800 V / cm. It is first kept at a nucleation temperature of 800°C for 2 h and then kept at a crystallization temperature of 940°C for 2 h. After cooling to room temperature, it is taken out and the surface of the glass ceramic is milled and polished to a thickness of 1.5 mm to prepare a transparent glass ceramic with a crystallization rate of 90%.

[0049] The transmittance curve and SEM of the transparent glass-ceramic prepared in this embodiment are similar to those in Embodiment 1, the grain size is 30-50 nm, and the Vickers hardness reaches 10.0 GPa.

[0050] Example 4

[0051] (1) Weighing glass powder raw materials The following raw materials were weighed according to the following mass percentages: ZnO 12wt%, MgO 12wt%, Al2O3 24wt%, SiO2 44wt%, Sb2O3 2wt%, nucleating agent TiO2 2wt%, nucleating agent ZrO2 2wt%, and nucleating agent P2O5 2wt%. The glass powder was ground for 3 h and mixed evenly. The mixture was added into a platinum-rhodium crucible, placed in a lifting furnace, heated at a rate of 10°C / min, and melted at 1680°C for 4 h to obtain glass liquid.

[0052] (2) pouring the glass liquid into a copper mold preheated to 500°C to form a transparent glass block;

[0053] (3) annealing the glass block at 780° C. for 10 h to obtain a precursor glass, and cutting and polishing the precursor glass to a glass thickness of 2 mm;

[0054] (4) The precursor glass was placed between the electrodes with an electric field strength of 700 V / cm. It was first kept at a nucleation temperature of 820°C for 2 h and then kept at a crystallization temperature of 960°C for 2 h. After cooling to room temperature, it was taken out and the surface of the glass ceramic was milled and polished to a thickness of 1.5 mm to obtain a transparent glass ceramic with a crystallization rate of 89%.

[0055] The transmittance curve and SEM of the transparent glass-ceramic prepared in this embodiment are similar to those in Embodiment 1, the grain size is 30-70 nm, and the Vickers hardness reaches 9.5 GPa.

[0056] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a transparent glass-ceramic with high hardness and high crystallinity, characterized in that: The following steps are involved: (1) weighing a glass powder raw material, grinding the glass powder for 0.5 to 2 hours, adding the glass powder into a platinum-rhodium crucible, and melting the glass powder at 1500 to 1750° C. for 2 to 4 hours to obtain a glass liquid; wherein the glass powder raw material is composed of the following components in weight percentage: ZnO 0 to 12 wt%, MgO 6 to 18 wt%, Al2O3 22 to 35 wt%, SiO2 40 to 50 wt%, Sb2O3 1 to 3 wt%, and a nucleating agent 0.5 to 9 wt%; (2) pouring the glass liquid into a preheated copper mold to obtain a transparent glass block; (3) annealing the glass block to obtain a precursor glass, and cutting and polishing the precursor glass, wherein the glass thickness is 2 mm; (4) The precursor glass is placed between the electrode sheets, first kept at a nucleation temperature of 700 to 900°C for 1 to 10 hours, then kept at a crystallization temperature of 900 to 1150°C for 2 to 8 hours, and then taken out after cooling to room temperature to prepare a transparent glass ceramic.

2. The method for preparing a high-hardness and high-crystallinity transparent glass-ceramic according to claim 1, characterized in that: In step (1), the heating rate of the lifting furnace is 5 to 20°C / min.

3. The method for preparing a transparent glass-ceramic with high hardness and high crystallinity according to claim 1, characterized in that: In step (1), the nucleating agent is selected from one or more of P2O5, ZrO2, TiO2, Eu2O3, and CeO2.

4. The method for preparing a transparent glass-ceramic with high hardness and high crystallinity according to claim 1, characterized in that: In step (2), the copper mold is preheated to a temperature of 300 to 600°C.

5. The method for preparing a transparent glass-ceramic with high hardness and high crystallinity according to claim 1, characterized in that: In step (4), the glass is annealed in air at 500-800° C. for 4-10 hours.

6. The method for preparing a transparent glass-ceramic with high hardness and high crystallinity according to claim 1, characterized in that: In step (4), the glass is placed between the positive and negative electrodes of the electrode sheet, and the electric field strength is 300 to 1000 V / cm. When the temperature in the furnace rises to the crystallization temperature, the power is turned on and maintained at the target electric field strength until the crystallization time ends.

7. The method for preparing a transparent glass-ceramic with high hardness and high crystallinity according to claim 1, characterized in that: Step (4) also includes milling and polishing the crystallized glass ceramic, and the thickness of the glass ceramic is 1.5 mm.

8. A transparent glass-ceramic with high hardness and high crystallinity obtained by the preparation method according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Arsenic-free spinel glass-ceramics with high visible transmission

    CN103298760A

  • Method for preparing glass ceramics

    CN106630569A

  • Glass ceramic and reinforced glass ceramic for front cover of 5G (fifth generation) mobile communication terminal

    CN108409147A

  • Glass ceramics and preparation method thereof

    CN110156334A

  • Preparation method of rare earth doped ZnAl2O4 nanocrystalline glass

    CN114133142A