Method for regulating and controlling crystal form of carbonized product and improving carbonization performance of low-carbon clinker

By using ionizable crystal form regulators of low-alkali metal ions and sulfate ions in low-carbon clinker, the carbonization reaction process is changed and the formation of aragonite is promoted, and the problem of CaCO3 crystal form regulation in low-carbon clinker is solved and the problem of improving the concentration of CaCO3 crystal form is improved. Carbonization performance and carbon sequestration rate reduce molding usage and cost.

CN119059749AActive Publication Date: 2024-12-03HUAXIN CEMENT CO LTD

Patent Information

Application Number
CN202411188300.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-03
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

The prior art is difficult to effectively regulate the crystal form of CaCO3 in low-carbon clinker, resulting in poor carbonization performance and easy carbonization reaction to produce calcite, affecting the carbonization strength and carbon sequestration rate.

Method used

The crystal form regulator of low alkaline metal ions and sulfate ions that can be ionized in water, such as MgSO4, changes the carbonization reaction process by promoting the dissolution and carbonization reaction of Ca2+, promotes the formation of aragonite, and increases the water retention agent MgCl2. Carbonization stability.

Benefits of technology

It significantly improves the carbonization strength and carbon sequestration rate of low-carbon clinker, promotes the formation of aragonite, improves the pore filling and connection effect, and reduces the molding usage and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005014207140000101
    Figure BDA0005014207140000101
  • Figure BDA0005014207140000111
    Figure BDA0005014207140000111
  • Figure BDA0005014207140000112
    Figure BDA0005014207140000112
Patent Text Reader

Abstract

The invention discloses a method for regulating and controlling the crystal form of a carbonized product and improving the carbonization performance of low-carbon clinker. The method comprises the following steps: 1) mixing the low-carbon clinker, a crystal form regulating and controlling agent and water, and carrying out compression molding; the crystal form regulating agent can ionize low-alkalinity metal ions and sulfate ions in water; and 2) drying the molded sample, and carbonizing to obtain a carbonized product. According to the method, the carbonization reaction process can be changed, the crystal form of CaCO3 in the carbonization product can be regulated and controlled, the formation of the aragonite crystal form is effectively promoted, the more effective filling and connecting effects on pores are achieved, continuous carbonization of the low-carbon clinker is facilitated, and on the premise that the forming dosage of the low-carbon clinker is reduced, the yield of the low-carbon clinker is increased. The carbonization strength and the carbon sequestration rate of the formed and carbonized low-carbon clinker can be effectively improved, and the method is suitable for different types of low-carbon clinker.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and in particular relates to a method for regulating the crystal form of carbonized products and improving the carbonization performance of low-carbon clinker. Background Art

[0002] Cement manufacturing is one of the world's largest sources of CO2 emissions, and CO2 emissions mainly come from the CO2 decomposed from limestone during cement production. CO2 emissions have become an indicator that must be strictly controlled in cement manufacturing. Compared with silicate cement clinker, low-carbon cement clinker (low-calcium cement clinker) requires less limestone and has a lower calcination temperature during burning, which can reduce CO2 emissions by about 20% during the production process. If the CO2 absorbed by low-carbon cement clinker after subsequent carbonization is taken into account (accounting for about 60% of theoretical carbon fixation), the total CO2 emissions can be reduced by about 50%. Therefore, low-carbon cement clinker has become a hot research topic in recent years.

[0003] The strength of low-carbon clinker is mainly formed by absorbing CO2 after molding to generate CaCO3 which fills the pores in the structure. There are three crystal forms of CaCO3 in the carbonization product, namely calcite, aragonite and vaterite. Among them, calcite and vaterite are spherical, granular and massive, while aragonite is needle-rod-shaped with a large aspect ratio. Therefore, it is believed that making the carbonization product aragonite can effectively improve the carbonization performance of low-carbon clinker. However, aragonite and vaterite are metastable and can be gradually converted into calcite (calcite is the most stable) in the presence of water.

[0004] Existing research usually uses chemical synthesis to prepare vaterite and aragonite. First, CaCl2 and (NH4)2CO3 are reacted under certain conditions to prepare vaterite, and then MgCl2 is added to convert vaterite into aragonite at 50-90℃. The reaction conditions need to be strictly controlled. However, low-carbon clinker needs to be formed and carbonized to form strength, which is affected by the forming method, CO2 diffusion, low-carbon clinker Ca 2+ Due to the influence of multiple factors such as dissolution rate, water dosage, temperature, CO2 concentration, etc., the concentration of each ion gradually changes during the carbonization process and cannot be effectively controlled; in addition, it is usually necessary to first consider the impact of carbonization conditions on the uniformity of carbonization and the final carbonization performance, and it is difficult to take into account the crystal form regulation of CaCO3 in the carbonization product; and the essence of the carbonization reaction of low-carbon clinker is an acid-base neutralization reaction, all of which lead to the easy formation of calcite after carbonization.

[0005] How to effectively regulate the crystal form of CaCO3 and improve the carbonization performance of low-carbon clinker under the complex carbonization conditions of low-carbon clinker has become a technical problem that needs to be solved urgently. Summary of the invention

[0006] The purpose of the present invention is to provide a method that can regulate the crystal form of carbonization products and improve the carbonization performance of low-carbon clinker, which can change the carbonization reaction process to regulate the crystal form of CaCO3 in the carbonization product, effectively promote the formation of aragonite, play a more effective filling and connecting role on the pores, and is beneficial to the continuous carbonization of low-carbon clinker. On the premise of reducing the amount of low-carbon clinker molding, the carbonization strength and carbon fixation rate of low-carbon clinker after carbonization are effectively improved, and the method is suitable for different types of low-carbon clinker.

[0007] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0008] A method for regulating the crystal form of carbonized products and improving the carbonization performance of low-carbon clinker comprises the following steps:

[0009] (1) mixing low-carbon clinker, a crystal form regulator and water, and pressing to form; the crystal form regulator can ionize low-alkalinity metal ions and sulfate ions in water;

[0010] (2) After the obtained molded sample is dried, it is carbonized to obtain a carbonized product.

[0011] According to the above scheme, the low-carbon clinker in step (1) is mainly composed of one or more of the common calcium silicate minerals βC2S, γC2S, C7MS4, C3S2, CS, C2AS, and C2MS2, and the mass ratio of CaO to SiO2 in the chemical composition of the low-carbon clinker is 0.8-1.9.

[0012] Preferably, the chemical components and their mass percentages in the low-carbon clinker include: CaO 42-59%, SiO2 30-47%, Al2O3 0-10%, Fe2O3 0-10%, and MgO 0-5%.

[0013] According to the above scheme, the crystal form regulator in step (1) includes at least one of MgSO4 and CuSO4, and other low-alkalinity metal ions (Mg) that can be ionized in water can also be used. 2+ and / or Cu 2+ ) and SO4 2- of substance.

[0014] According to the above scheme, the amount of the crystal form regulator in step (1) is 0.5-5wt% of the amount of low-carbon clinker.

[0015] Preferably, in addition to the crystal form regulator, MgCl2 accounting for 0.5-5wt% of the amount of low-carbon clinker can be added as a water retaining agent to improve carbonization stability.

[0016] According to the above scheme, the amount of water used in step (1) is 10-25wt% of the amount of low-carbon clinker used.

[0017] According to the above scheme, in step (2), the moisture content after drying is 4-20wt%.

[0018] Furthermore, in step (2), the sample is dried at a temperature of 20-50°C.

[0019] According to the above scheme, the carbonization conditions include: CO2 concentration 15-100%, temperature 20-50°C, humidity 40-80%, and pressurization pressure 0-0.3MPa.

[0020] According to the above scheme, the carbonization time is 6-72h.

[0021] The carbonized product prepared according to the above scheme has an aragonite content of more than 6.5 wt % and an aragonite average particle size of more than 24 nm.

[0022] Preferably, the aragonite content in the obtained carbonized product is greater than 15 wt%.

[0023] Furthermore, the carbonization strength of the carbonized product prepared according to the above scheme can be increased by 10-30%, and the carbon fixation rate can be increased by 10-60% compared with the condition without adding the crystal form regulator.

[0024] The principle of the present invention is:

[0025] The essence of the carbonization reaction of low-carbon clinker is that the low-carbon clinker dissolves alkaline Ca(OH)2 or alkaline calcium silicate hydrate, and reacts with H2CO3 to produce CaCO3 by acid-base neutralization reaction; the reaction is easy to occur and is an exothermic reaction. The present invention adopts a crystal form regulator suitable for low-carbon clinker molding and carbonization, which can be ionized into low-alkaline cations (Mg 2+ or Cu 2+ etc.) and SO4 2- Taking MgSO4 as an example, the mechanism of the influence of anions on the carbonization of low-carbon clinker is the following reactions 1 to 4:

[0026] Reaction 1 is that MgSO4 promotes the Ca in low carbon clinker 2+ Dissolved as CaSO4·2H2O which is slightly soluble in water:

[0027] MgSO4+CaO·xSiO2+yH2O→Mg(OH)2·xSiO2·(y-3)H2O+CaSO4·2H2O

[0028] Reaction 2 is the dissolution of CO2 in water:

[0029] CO2+H2O→H2CO3

[0030] Reaction 3 is the carbonization of Mg(OH)2 to Mg(HCO3)2:

[0031] Mg(OH)2·xSiO2·(y-3)H2O+2H2CO3+H2O→Mg(HCO3)2+xSiO2·yH2O

[0032] Reaction 4 is the carbonization of CaSO4·2H2O by Mg(HCO3)2 to CaCO3 and reformation of MgSO4:

[0033] Mg(HCO3)2+CaSO4·2H2O→CaCO3+CO2+3H2O+MgSO4

[0034] (1) The crystal form regulator MgSO4 can be recycled and only acts as a reaction aid in carbonization. It generates slightly soluble Mg(OH)2 silica gel complex and slightly soluble CaSO4·2H2O through reaction 1, which can accelerate and continuously promote the Ca2+ removal in low-carbon clinker. 2+ The dissolution of Mg(HCO3)2 can be carried out through reactions 2, 3, and 4 to carbonize the Mg(HCO3)2, effectively increasing the carbonizable amount of low-carbon clinker.

[0035] (2) The water content of low-carbon clinker during carbonization is much less than that of CaCO3 synthesized by chemical synthesis, and the alkalinity of Ca(OH)2 is relatively strong, which makes Ca in water 2+ OH - The concentration is relatively high, and the carbonization reaction of low-carbon clinker is essentially an acid-base neutralization reaction, which leads to a fast rate of CaCO3 generation and a high degree of supersaturation, and calcite is easily generated after carbonization. Although the acid-base neutralization reaction has the highest priority and the fastest reaction in the double decomposition reaction, the double decomposition reaction of the crystal form regulator cannot be completely prevented because of the low solubility and weak acidity of H2CO3 and the insufficient amount of H2CO3 in water relative to the low-carbon clinker, which is consumed and affected by diffusion. Through reactions 1 to 4, the acid-base neutralization reaction is changed into a double decomposition reaction without acid-base neutralization, and the slightly soluble CaSO4·2H2O is generated, which reduces the alkalinity of the reaction system and further reduces the Ca in water. 2+ The concentration of Ca dissolved by the crystal modifier 2 + It cannot be carbonized directly by H2CO3, but can only be carbonized by Mg(HCO3)2 generated through reactions 2, 3, and 4, which slows down the rate of CaCO3 generated by the crystal form regulator and reduces the supersaturation, thereby promoting the formation of aragonite.

[0036] (3) The addition of the crystal modifier changes the carbonization reaction from an acid-base neutralization reaction to a non-acid-base neutralization double decomposition reaction, which not only promotes the degradation of Ca in low-carbon clinker, but also promotes the degradation of Ca in low-carbon clinker. 2+ The dissolution of Ca 2+ The carbonization rate of this part of Ca 2+It can be better transported with water, so that CaCO3 is generated in the pores on the surface of non-low-carbon clinker, and aragonite with a large aspect ratio is generated, which plays a more effective role in filling and connecting the pores, which is beneficial to the continuous carbonization of low-carbon clinker;

[0037] (4) For Ca itself 2+ Low carbon clinker with slow dissolution rate (low calcium-silicon ratio is lower than that of low carbon clinker with high calcium-silicon ratio) 2+ The dissolution rate is slower, the carbonization rate is slower), the effect of the crystal form regulator is more obvious, and more aragonite can be generated;

[0038] (5) Since reaction 1 is easily generated when low carbon clinker is pressed and formed to produce CaSO4·2H2O, the compactness of the low carbon clinker will be reduced, thereby reducing the water retention. Therefore, a certain amount of water retaining agent (MgCl2) can be compounded in the crystal form regulator. However, the solubility of CaCl2 generated by reaction 1 of MgCl2 alone is high, which makes the rate of reaction 1 slower than that of MgSO4, and it will not promote the formation of aragonite, and cannot achieve the effect of MgSO4.

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] 1) The present invention uses sulfate of low alkaline metal (Mg and / or Cu) as a crystal form regulator and applies it to the carbonization process of low carbon clinker to promote the carbonization of Ca in low carbon clinker. 2+ dissolution, while reducing the alkalinity of the reaction system and reducing the dissolved Ca 2+ The carbonization rate of this part of Ca 2+ It can be better transported with water, so that CaCO3 is generated in the pores on the surface of non-low-carbon clinker, and promotes the formation of aragonite with a large aspect ratio, which plays a more effective role in filling and connecting the pores, is conducive to the continuous carbonization of low-carbon clinker, effectively improves the carbonization strength and carbon fixation rate of low-carbon clinker after molding and carbonization, and can significantly reduce the amount of low-carbon clinker in the product, thereby reducing costs, providing a new idea for the preparation of high-performance carbonized products;

[0041] 2) The preparation method involved in the present invention is relatively simple, easy to operate, has wide applicability to low-carbon clinker, and is suitable for promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 The XRD diagrams of the carbonized products obtained in Examples 1 to 5 and Comparative Example 1;

[0043] Figure 2 The XRD diagrams of the carbonized products obtained in Comparative Examples 4 to 6 and 8 to 10;

[0044] Figure 3 The XRD patterns of the carbonized products obtained in Examples 6 and 7 and Comparative Examples 2, 3 and 7 are shown;

[0045] Figure 4 This is the SEM image of the carbonized product obtained in Example 1. DETAILED DESCRIPTION

[0046] The present invention is not limited to the above-mentioned embodiments. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications are also considered to be within the scope of protection of the present invention. The contents not described in detail in this specification belong to the prior art known to professional and technical personnel in this field.

[0047] The following are the low-carbon clinker and chemical reagents used in the specific embodiments:

[0048] Different types of low-carbon clinker are obtained. The chemical composition and mineral composition of the low-carbon clinker used in the embodiment of the present invention are shown in Table 1 and Table 2, respectively, and the low-carbon clinker is ground to R45μm≤20% before use.

[0049] Table 1 Chemical composition of low carbon clinker (%)

[0050] name CaO <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> MgO Low carbon clinker 1 56.95 32.11 3.10 1.87 3.08 Low carbon clinker 2 49.98 39.81 3.07 2.35 2.10 Low carbon clinker 3 42.33 46.86 3.27 2.58 1.73

[0051] Table 2 Mineral composition of low carbon clinker (%)

[0052] name <![CDATA[βC2S]]> <![CDATA[C7MS4]]> <![CDATA[C3S2]]> CS <![CDATA[C2AS]]> <![CDATA[C2MS2]]> <![CDATA[SiO2]]> Low carbon clinker 1 38.8 52.4 0 0 6.2 2.7 0 Low carbon clinker 2 8.0 0 56.7 15.6 4.4 13.8 1.6 Low carbon clinker 3 0 0 0 83.3 2.0 8.3 6.3

[0053] The mass ratios of CaO to SiO2 (i.e., the mass ratio of calcium to silicon) in the chemical composition of low carbon clinkers 1, 2, and 3 are 1.77, 1.26, and 0.90, respectively.

[0054] In the following examples and comparative examples, the chemical reagents used are analytically pure MgSO4, analytically pure CuSO4·5H2O, analytically pure MgCl2·6H2O, analytically pure Na2SO4, analytically pure FeSO4, and analytically pure Mg(HCO3)2.

[0055] Example 1

[0056] A method for regulating the crystal form of carbonized products and improving the carbonization performance of low-carbon clinker comprises the following steps:

[0057] 1. Ratio

[0058] Weigh 1 100 parts of low carbon clinker, 2 parts of analytical pure MgSO4, and 15 parts of water;

[0059] 2. Sample preparation

[0060] First, weighed water and MgSO4 were put into a mixer and stirred until MgSO4 was completely dissolved in the water. Then, low-carbon clinker 1 was added and stirred for 1 minute. The mixed wet material was pressed into a cylindrical sample with a diameter of 2 cm and a height of 2 cm at a molding pressure of 10 MPa. The mass of the sample was 13.9 g. The mass of low-carbon clinker 1 contained in the sample (molding amount, the same below) was calculated to be 11.88 g according to 13.9 g*100 g / (100 g+15 g+2 g).

[0061] 3. Pre-drying and carbonization

[0062] The sample was dried under natural conditions to a moisture content of 9% (the moisture content with the highest carbonization strength obtained according to the carbonization test after drying to different moisture contents), and finally carbonized for 20 hours under the conditions of a carbon dioxide concentration of 99%, a temperature of 30°C, a humidity of 60%, and an air pressure of 0.3MPa (pressure indication 0.3MPa) to obtain a carbonized product.

[0063] Example 2

[0064] A method for regulating the crystal form of carbonized products and improving the carbonization performance of low-carbon clinker comprises the following steps:

[0065] 1. Ratio

[0066] Weigh 1 100 parts of low carbon clinker, 1 part of analytical pure MgSO4, and 15 parts of water;

[0067] 2. Sample preparation

[0068] First, weighed water and MgSO4 were put into a mixer and stirred until MgSO4 was completely dissolved in the water. Then, low-carbon clinker 1 was added and stirred for 1 minute. The mixed wet material was pressed into a cylindrical sample with a diameter of 2 cm and a height of 2 cm at a molding pressure of 10 MPa. The mass of the sample was 14.4 g. The mass of low-carbon clinker 1 contained in the sample was calculated to be 12.41 g according to 14.4 g*100 g / (100 g+15 g+1 g).

[0069] 3. Pre-drying and carbonization

[0070] The sample was dried under natural conditions to a moisture content of 9% (the moisture content with the highest carbonization strength obtained according to the carbonization test after drying to different moisture contents), and finally carbonized for 20 hours under the conditions of a carbon dioxide concentration of 99%, a temperature of 30°C, a humidity of 60%, and an air pressure of 0.3MPa (pressure indication 0.3MPa) to obtain a carbonized product.

[0071] Example 3

[0072] A method for regulating the crystal form of carbonized products and improving the carbonization performance of low-carbon clinker comprises the following steps:

[0073] 1. Ratio

[0074] Weigh 1 100 parts of low carbon clinker, 3 parts of analytical pure MgSO4, and 15 parts of water;

[0075] 2. Sample preparation

[0076] First, weighed water and MgSO4 were put into a mixer and stirred until MgSO4 was completely dissolved in the water. Then, low-carbon clinker 1 was added and stirred for 1 minute. The mixed wet material was pressed into a cylindrical sample with a diameter of 2 cm and a height of 2 cm at a molding pressure of 10 MPa. The mass of the sample was 13.7 g. The mass of low-carbon clinker 1 contained in the sample was calculated to be 11.61 g according to 13.7 g*100 g / (100 g+15 g+3 g).

[0077] 3. Pre-drying and carbonization

[0078] The sample was dried under natural conditions to a moisture content of 10% (the moisture content with the highest carbonization strength obtained from the carbonization test after drying to different moisture contents), and finally carbonized for 20 hours under the conditions of a carbon dioxide concentration of 99%, a temperature of 30°C, a humidity of 60%, and an air pressure of 0.3MPa (pressure indication 0.3MPa) to obtain a carbonized product.

[0079] Example 4

[0080] A method for regulating the crystal form of carbonized products and improving the carbonization performance of low-carbon clinker comprises the following steps:

[0081] 1. Ratio

[0082] Weigh 1,100 parts of low-carbon clinker, 2 parts of analytically pure MgSO4, 2 parts of analytically pure MgCl2·6H2O, and 13.9 parts of water (15-2*108 / 203, according to the calculation, the water introduced in the analytically pure MgCl2·6H2O is taken into account to ensure that the total amount of water is 15 parts);

[0083] 2. Sample preparation

[0084] First, weighed water, MgSO4 and MgCl2·6H2O were put into a mixer and stirred until MgSO4 and MgCl2·6H2O were completely dissolved in the water. Then, low-carbon clinker 1 was added and stirred for 1 min. The mixed wet material was pressed into a cylindrical sample with a diameter of 2 cm and a height of 2 cm at a molding pressure of 10 MPa. The mass of the sample was 13.7 g. The mass of low-carbon clinker 1 contained in the sample was calculated to be 11.62 g according to 13.7 g*100 g / (100 g+13.9 g+2 g+2 g).

[0085] 3. Pre-drying and carbonization

[0086] The sample was dried under natural conditions to a moisture content of 10% (the moisture content with the highest carbonization strength obtained from the carbonization test after drying to different moisture contents), and finally carbonized for 20 hours under the conditions of a carbon dioxide concentration of 99%, a temperature of 30°C, a humidity of 60%, and an air pressure of 0.3MPa (pressure indication 0.3MPa) to obtain a carbonized product.

[0087] Example 5

[0088] A method for regulating the crystal form of carbonized products and improving the carbonization performance of low-carbon clinker comprises the following steps:

[0089] 1. Ratio

[0090] Weigh 1,100 parts of low-carbon clinker, 4 parts of analytically pure CuSO4·5H2O, 2 parts of analytically pure MgCl2·6H2O, and 12.5 parts of water (15-4*90 / 249.5-2*108 / 203, according to the calculation, the water introduced by analytically pure CuSO4·5H2O and analytically pure MgCl2·6H2O is considered to ensure that the total amount of water is 15 parts);

[0091] 2. Sample preparation

[0092] First, weighed water, CuSO4·5H2O and MgCl2·6H2O were put into a mixer and stirred until CuSO4·5H2O and MgCl2·6H2O were completely dissolved in the water. Then, low-carbon clinker 1 was added and stirred for 1 min. The mixed wet material was pressed into a cylindrical sample with a diameter of 2 cm and a height of 2 cm at a molding pressure of 10 MPa. The mass of the sample was 13.6 g. The mass of low-carbon clinker 1 contained in the sample was calculated to be 11.48 g according to 13.6 g*100 g / (100 g+12.5 g+4 g+2 g).

[0093] 3. Pre-drying and carbonization

[0094] The sample was dried under natural conditions to a moisture content of 10% (the moisture content with the highest carbonization strength obtained from the carbonization test after drying to different moisture contents), and finally carbonized for 20 hours under the conditions of a carbon dioxide concentration of 99%, a temperature of 30°C, a humidity of 60%, and an air pressure of 0.3MPa (pressure indication 0.3MPa) to obtain a carbonized product.

[0095] Example 6

[0096] A method for regulating the crystal form of carbonized products and improving the carbonization performance of low-carbon clinker comprises the following steps:

[0097] 1. Ratio

[0098] Weigh 2 100 parts of low-carbon clinker, 2 parts of analytically pure MgSO4, 2 parts of analytically pure MgCl2·6H2O, and 18.9 parts of water (20-2*108 / 203, according to the calculation, the water introduced in the analytically pure MgCl2·6H2O is taken into account to ensure that the total amount of water is 20 parts);

[0099] 2. Sample preparation

[0100] First, weighed water, MgSO4 and MgCl2·6H2O were put into a mixer and stirred until MgSO4 and MgCl2·6H2O were completely dissolved in the water. Then, low-carbon clinker 2 was added and stirred for 1 min. The mixed wet material was pressed into a cylindrical sample with a diameter of 2 cm and a height of 2 cm at a molding pressure of 10 MPa. The mass of the sample was 12.6 g. The mass of low-carbon clinker 2 contained in the sample was calculated to be 10.25 g according to 12.6 g*100 g / (100 g+18.9 g+2 g+2 g).

[0101] 3. Pre-drying and carbonization

[0102] The sample was dried under natural conditions to a moisture content of 14% (the moisture content with the highest carbonization strength obtained according to the carbonization test after drying to different moisture contents), and finally carbonized for 20 hours under the conditions of a carbon dioxide concentration of 99%, a temperature of 30°C, a humidity of 60%, and an air pressure of 0.3MPa (pressure indication 0.3MPa) to obtain a carbonized product.

[0103] Example 7

[0104] A method for regulating the crystal form of carbonized products and improving the carbonization performance of low-carbon clinker comprises the following steps:

[0105] 1. Ratio

[0106] Weigh 3 100 parts of low-carbon clinker, 2 parts of analytically pure MgSO4, 2 parts of analytically pure MgCl2·6H2O, and 18.9 parts of water (20-2*108 / 203, according to the calculation, the water introduced in the analytically pure MgCl2·6H2O is considered to ensure that the total amount of water is 20 parts);

[0107] 2. Sample preparation

[0108] First, weighed water, MgSO4 and MgCl2·6H2O were put into a mixer and stirred until MgSO4 and MgCl2·6H2O were completely dissolved in the water. Then, low-carbon clinker 3 was added and stirred for 1 minute. The mixed wet material was pressed into a cylindrical sample with a diameter of 2 cm and a height of 2 cm at a molding pressure of 10 MPa. The mass of the sample was 12.6 g. The mass of low-carbon clinker 3 contained in the sample was calculated to be 10.25 g according to 12.6 g*100 g / (100 g+18.9 g+2 g+2 g).

[0109] 3. Pre-drying and carbonization

[0110] The sample was dried under natural conditions to a moisture content of 14% (the moisture content with the highest carbonization strength obtained according to the carbonization test after drying to different moisture contents), and finally carbonized for 20 hours under the conditions of a carbon dioxide concentration of 99%, a temperature of 30°C, a humidity of 60%, and an air pressure of 0.3MPa (pressure indication 0.3MPa) to obtain a carbonized product.

[0111] Comparative Example 1

[0112] A low-carbon clinker carbonization process, the preparation method of which is substantially the same as that of Example 1, except that no crystal form regulator is introduced, and the specific steps include the following:

[0113] Weigh 1100 parts of low-carbon clinker 1 and 15 parts of water, and press and mold them in the same way (to form a cylindrical sample with the same specifications as in Example 1). The mass of the sample is 14.8 g. According to 14.8g*100g / (100g+15g), it can be calculated that the mass of low-carbon clinker 1 contained in the sample is 12.9 g (higher than the molding amount described in Example 1). The sample is then dried under natural conditions to a moisture content of 7% (the moisture content with the highest carbonization strength obtained from the carbonization test after drying to different moisture contents). Finally, it is carbonized for 20 hours under the conditions of a carbon dioxide concentration of 99%, a temperature of 30°C, a humidity of 60%, and an air pressure of 0.3 MPa (pressure indication 0.3 MPa) to obtain a carbonized product.

[0114] Comparative Example 2

[0115] A low-carbon clinker carbonization process, the preparation method of which is substantially the same as that of Example 6, except that no crystal form regulator is introduced, and the specific steps include the following:

[0116] Weigh 100 parts of low-carbon clinker 2 and 20 parts of water, and press into shape using the same method. The mass of the sample is 13.0 g. The mass of the low-carbon clinker 2 contained in the sample is calculated to be 10.8 g according to 13.0 g*100 g / (100 g+20 g). Then dry the sample under natural conditions to a moisture content of 16% (the moisture content with the highest carbonization intensity obtained from the carbonization test after drying to different moisture contents). Finally, carbonize it for 20 hours under the conditions of a carbon dioxide concentration of 99%, a temperature of 30°C, a humidity of 60%, and an air pressure of 0.3 MPa (pressure indication 0.3 MPa) to obtain a carbonized product.

[0117] Comparative Example 3

[0118] A low-carbon clinker carbonization process, the preparation method of which is substantially the same as that of Example 7, except that no crystal form regulator is introduced, and the specific steps include the following:

[0119] Weigh 100 parts of low-carbon clinker 3 and 20 parts of water, and press into shape using the same method. The mass of the sample is 12.8 g. The mass of the low-carbon clinker 3 contained in the sample can be calculated based on 12.8 g*100 g / (100 g+20 g), which is 10.7 g. The sample is then dried under natural conditions to a moisture content of 16% (the moisture content with the highest carbonization intensity obtained from the carbonization test after drying to different moisture contents). Finally, it is carbonized for 20 hours under the conditions of a carbon dioxide concentration of 99%, a temperature of 30°C, a humidity of 60%, and an air pressure of 0.3 MPa (pressure indication 0.3 MPa) to obtain a carbonized product.

[0120] Comparative Example 4

[0121] A low-carbon clinker carbonization process, the preparation method of which is substantially the same as that of Example 1, the components and their weight proportions are: 1 100 parts of low-carbon clinker, analytically pure MgCl2·6H2O 2 parts, 13.9 parts of water (15-2*108 / 203, according to the calculation, the water introduced in the analytical pure MgCl2·6H2O is considered to ensure that the total amount of water is 15 parts), and the specific steps include: after pressing and molding by the same method, the mass of the sample is weighed to be 14.7g, and the mass of the low-carbon clinker 1 contained in the sample can be calculated according to 14.7g*100g / (100g+13.9g+2g) to be 12.68g (higher than the molding amount described in Example 1), and then the sample is dried under natural conditions to a moisture content of 7% (the moisture content with the highest carbonization strength obtained according to the carbonization test after drying to different moisture contents), and finally carbonized for 20 hours under the conditions of a carbon dioxide concentration of 99%, a temperature of 30°C, a humidity of 60%, and an air pressure of 0.3MPa (pressure indication number 0.3MPa) to obtain a carbonized product.

[0122] Comparative Example 5

[0123] A low-carbon clinker carbonization process, the preparation method of which is substantially the same as that of Example 1, the components and their weight proportions are: 1 100 parts of low-carbon clinker, analytically pure MgCl2·6H2O 4 parts, 12.9 parts of water (15-4*108 / 203, according to the calculation, the water introduced in the analytical pure MgCl2·6H2O is considered to ensure that the total amount of water is 15 parts), and the specific steps include: after pressing and molding by the same method, the mass of the sample is weighed to be 14.7g, and the mass of the low-carbon clinker 1 contained in the sample can be calculated according to 14.7g*100g / (100g+12.9g+4g) to be 12.57g (higher than the molding amount described in Example 1), and then the sample is dried under natural conditions to a moisture content of 7% (the moisture content with the highest carbonization strength obtained according to the carbonization test after drying to different moisture contents), and finally carbonized for 20 hours under the conditions of carbon dioxide concentration of 99%, temperature of 30°C, humidity of 60%, and air pressure of 0.3MPa (pressure indication number 0.3MPa) to obtain a carbonized product.

[0124] Comparative Example 6

[0125] A low-carbon clinker carbonization process, the preparation method of which is substantially the same as that of Example 1, the components and their weight proportions are: 1 100 parts of low-carbon clinker, analytically pure MgCl2·6H2O 6 parts, 11.8 parts of water (15-6*108 / 203, according to the calculation, the water introduced in the analytical pure MgCl2·6H2O is considered to ensure that the total amount of water is 15 parts), and the specific steps include: after pressing and molding by the same method, the mass of the sample is weighed to be 14.7g, and the mass of the low-carbon clinker 1 contained in the sample can be calculated according to 14.7g*100g / (100g+11.8g+6g) to be 12.48g (higher than the molding amount described in Example 1), and then the sample is dried under natural conditions to a moisture content of 7% (the moisture content with the highest carbonization strength obtained according to the carbonization test after drying to different moisture contents), and finally carbonized for 20 hours under the conditions of carbon dioxide concentration of 99%, temperature of 30°C, humidity of 60%, and air pressure of 0.3MPa (pressure indication number 0.3MPa) to obtain a carbonized product.

[0126] Comparative Example 7

[0127] A low-carbon clinker carbonization process, the preparation method of which is substantially the same as that of Example 6, the components and their weight proportions are: 2 100 parts of low-carbon clinker, analytically pure MgCl2·6H2O 4 parts, 17.9 parts of water (20-4*108 / 203, according to the calculation, the water introduced in the analytical pure MgCl2·6H2O is considered to ensure that the total amount of water is 20 parts), and the specific steps include: after pressing and molding by the same method, the mass of the sample is weighed to be 13.1g, and the mass of the low-carbon clinker 2 contained in the sample can be calculated according to 13.1g*100g / (100g+17.9g+4g) to be 10.75g, and then the sample is dried under natural conditions to a moisture content of 11% (the moisture content with the highest carbonization intensity obtained according to the carbonization test after drying to different moisture contents), and finally carbonized for 20h under the conditions of carbon dioxide concentration of 99%, temperature of 30°C, humidity of 60%, and air pressure of 0.3MPa (pressure indication number 0.3MPa) to obtain a carbonized product.

[0128] Comparative Example 8

[0129] A low-carbon clinker carbonization process, whose preparation method is roughly the same as that of Example 1, and the components and their weight proportions are: 1100 parts of low-carbon clinker 1, 2 parts of analytical pure Na2SO4, and 15 parts of water. The specific steps include: after pressing and molding by the same method, the mass of the sample is weighed to be 14.8g, and the mass of the low-carbon clinker 1 contained in the sample can be calculated according to 14.8g*100g / (100g+15g+2g) to be 12.65g (higher than the molding amount described in Example 1), and then the sample is dried under natural conditions to a moisture content of 9% (the moisture content with the highest carbonization strength obtained according to the carbonization test after drying to different moisture contents), and finally carbonized for 20 hours under the conditions of a carbon dioxide concentration of 99%, a temperature of 30°C, a humidity of 60%, and an air pressure of 0.3MPa (pressure indication number 0.3MPa) to obtain a carbonized product.

[0130] Comparative Example 9

[0131] A low-carbon clinker carbonization process, whose preparation method is roughly the same as that of Example 1, and the components and their weight proportions are: 1100 parts of low-carbon clinker 1, 2 parts of analytically pure FeSO4, and 15 parts of water. The specific steps include: after pressing and molding by the same method, the mass of the sample is weighed to be 14.1g, and the mass of the low-carbon clinker 1 contained in the sample can be calculated according to 14.1g*100g / (100g+15g+2g) to be 12.05g (higher than the molding amount described in Example 1), and then the sample is dried under natural conditions to a moisture content of 9% (the moisture content with the highest carbonization strength obtained according to the carbonization test after drying to different moisture contents), and finally carbonized for 20 hours under the conditions of a carbon dioxide concentration of 99%, a temperature of 30°C, a humidity of 60%, and an air pressure of 0.3MPa (pressure indication number 0.3MPa) to obtain a carbonized product.

[0132] Comparative Example 10

[0133] A low-carbon clinker carbonization process, whose preparation method is roughly the same as that of Example 1, and the components and their weight proportions are: 1100 parts of low-carbon clinker 1, 2 parts of analytically pure Mg(HCO3)2, and 15 parts of water. The specific steps include: after pressing and molding by the same method, the mass of the sample is weighed to be 14.6g, and the mass of the low-carbon clinker 1 contained in the sample can be calculated according to 14.6g*100g / (100g+15g+2g) to be 12.48g (higher than the molding amount described in Example 1), and then the sample is dried under natural conditions to a moisture content of 7% (the moisture content with the highest carbonization strength obtained according to the carbonization test after drying to different moisture contents), and finally carbonized for 20 hours under the conditions of a carbon dioxide concentration of 99%, a temperature of 30°C, a humidity of 60%, and an air pressure of 0.3MPa (pressure indication number 0.3MPa) to obtain a carbonized product.

[0134] After carbonization, jade was used to perform quantitative mineral composition analysis on the XRD patterns of each embodiment and comparative example and grain size analysis of CaCO3. The results are shown in Table 3 and Table 4, respectively.

[0135] Table 3 Mineral composition after carbonization (%)

[0136]

[0137]

[0138] Table 4 Average grain size of CaCO3 (nm)

[0139]

[0140]

[0141] Among them, the contents of aragonite and vaterite in some embodiments and comparative examples in Table 1 are relatively small, and the detection error is relatively large, which is not conducive to the effective determination of the corresponding average grain size, and is represented by " / ".

[0142] The compressive strength of the sample after carbonization is the carbonization strength. The carbonization strength and carbon fixation rate of each embodiment and comparative example after carbonization are shown in Table 5.

[0143] Table 5 Carbonization intensity and carbon fixation rate

[0144] project Carbonization strength / MPa Carbon fixation rate / % Example 1 176.12 23.27 Example 2 168.77 19.96 Example 3 187.61 25.84 Example 4 183.79 26.13 Example 5 179.44 25.22 Example 6 152.57 28.89 Example 7 110.61 21.26 Comparative Example 1 151.87 17.04 Comparative Example 2 130.32 25.41 Comparative Example 3 87.42 18.65 Comparative Example 4 168.32 19.20 Comparative Example 5 167.97 18.54 Comparative Example 6 158.61 18.60 Comparative Example 7 132.32 26.09 Comparative Example 8 120.83 15.53 Comparative Example 9 138.11 20.97 Comparative Example 10 125.06 17.93

[0145] The results show that for relatively complex low-carbon clinker forming carbonization, the introduction of low-alkaline cations and SO4 2- Anionic crystal form regulators are beneficial to increase the amount of aragonite generated, such as MgSO4, CuSO4, and FeSO4 used in the present invention, but the effects are MgSO4>CuSO4>FeSO4 from large to small, which is related to their own metal cation characteristics and the circulation efficiency of reactions 1 to 4, which leads to the poor effect of comparative example 9. The grain size of CaCO3 obtained by XRD analysis of jade represents the average grain size. After adding the crystal form regulator, the average grain size of the generated aragonite is larger than that of calcite. In addition, aragonite is needle-shaped, and the size of the long axis will be more obviously larger than that of calcite, which plays a more effective role in filling and connecting the pores.

[0146] For low-carbon clinker 1 with a high calcium-silicon mass ratio: the carbonization strength and carbon fixation rate of Examples 1, 2, 3, 4, and 5 with the addition of crystal form regulators are significantly improved compared with those of Comparative Example 1 without the addition of crystal form regulators; for low-carbon clinker 2 with a moderate calcium-silicon mass ratio: the carbonization strength and carbon fixation rate of Example 6 with the addition of crystal form regulators are significantly improved compared with those of Comparative Example 2 without the addition of crystal form regulators; for low-carbon clinker 3 with a low calcium-silicon mass ratio: the carbonization strength and carbon fixation rate of Example 7 with the addition of crystal form regulators are significantly improved compared with those of Comparative Example 3 without the addition of crystal form regulators. Among them, the lower the calcium-silicon mass ratio of low-carbon clinker, the easier it is to generate aragonite after adding the crystal form regulator, and the proportion of aragonite in the total amount of CaCO3 is higher, the grain size is large, the CO2 emission is low during the production of low-calcium-silicon ratio low-carbon clinker, the carbonization rate is slow, the adaptability to carbonization conditions is good (such as carbonization with a 20% CO2 concentration), the specific gravity is small, the amount of low-carbon clinker of the same molding volume is small (less molding amount), the molding volume of the same amount of low-carbon clinker is larger, and it is more suitable for casting molding carbonization and occasions requiring low product density. Secondly, the addition of crystal form regulators significantly reduces the molding amount of low-carbon clinker, and the cost of the required low-carbon clinker is lower.

[0147] In Comparative Examples 4, 5, 6, and 7, only MgCl2 was added, and the acid-base neutralization reaction of carbonization can also be changed into a double decomposition reaction without acid-base neutralization. However, the solubility of CaCl2 generated by MgCl2 through reaction 1 is high, so that the rate of reaction 1 is slower than that of MgSO4, which is not conducive to the formation of aragonite (the aragonite content is reduced relative to that of Comparative Example 1 without adding a crystal form regulator). The improvement effect and potential of carbonization strength and carbon fixation rate are significantly lower than those of MgSO4 obtained in the present invention. Although only MgCl2 was added in Comparative Examples 4 and 5, compared with Comparative Example 1, the molding amount of a small amount of low-carbon clinker was reduced and the amount of calcite generated after carbonization was increased, thereby improving the carbonization performance, which was close to the performance of Example 2 added with 1% MgSO4, but the improvement of the carbonization performance was limited. After further increasing the amount of MgCl2, Comparative Example 6 reduced the carbonization performance. The main reason is that increasing the amount of MgCl2 will not significantly reduce the molding amount of low-carbon clinker, will not promote the formation of aragonite, and the water retention is too strong. The time required for drying to a suitable moisture content is too long and too much reaction 1 occurs, resulting in poor moisture uniformity and volume stability of the sample before carbonization.

[0148] In Comparative Example 8, Na2SO4 is added. Since the NaOH generated by reaction 1 has high solubility and strong alkalinity, the rate of reaction 1 is slower than that of MgSO4 (the mass of the low-carbon clinker 1 contained in the sample of Comparative Example 8 does not change compared with that of Comparative Example 1, and the compactness of the molding does not change, which also shows the correctness of this view). In addition, it will accelerate the dissolution of CO2 in water and form Na2CO3 and NaHCO3, increase the alkalinity of the reaction system, and accelerate the rate at which CaSO4·2H2O and Ca(OH)2 are carbonized, but it cannot effectively promote the formation of aragonite. 2+ It also cannot be transported well with water, which easily causes CaCO3 to form on the surface of low-carbon clinker, which in turn reduces the carbonization intensity and carbon fixation rate.

[0149] In Comparative Example 10, Mg(HCO3)2 is added. Since Ca(HCO3)2 is directly generated through Reaction 1, and Ca(HCO3)2 is unstable and will decompose into CaCO3 above 0°C, this is equivalent to the reaction of Mg(HCO3)2 with the alkaline Ca(OH)2 to generate CaCO3, which will not promote the formation of aragonite and is equivalent to the Ca(OH)2 of low-carbon clinker. 2+ After dissolution, it is immediately carbonized, Ca 2+ It cannot be well transported with water, which easily causes CaCO3 to be generated on the surface of low-carbon clinker. Although the molding density is reduced to ensure that the carbon fixation rate is not reduced, the carbonization strength is significantly reduced.

[0150] The above-mentioned embodiments are only preferred embodiments of the present invention and cannot be used to limit the scope of protection of the present invention. Any non-substantial changes and substitutions made by technicians in this field on the basis of the present invention shall fall within the scope of protection required by the present invention.

Claims

1. A method for regulating the crystal form of carbonized products and improving the carbonization performance of low-carbon clinker, characterized in that: The following steps are involved: (1) mixing low-carbon clinker, a crystal form regulator and water, and pressing to form; the crystal form regulator can ionize low-alkalinity metal ions and sulfate ions in water; (2) After the obtained molded sample is dried, it is carbonized to obtain a carbonized product.

2. The method according to claim 1, characterized in that The low-carbon clinker in step (1) is mainly composed of one or more of βC2S, γC2S, C7MS4, C3S2, CS, C2AS, and C2MS2; the mass ratio of CaO to SiO2 in the chemical composition of the low-carbon clinker is 0.8-1.

9.

3. The method according to claim 1, characterized in that The low alkalinity metal ion is Mg 2+ , Cu 2+ One or more of the following.

4. The method according to claim 1, characterized in that The amount of the crystal form regulator in step (1) is 0.5-5wt% of the amount of low carbon clinker.

5. The method according to claim 1, characterized in that The amount of water used in step (1) is 10-25wt% of the amount of low-carbon clinker used.

6. The method according to claim 1, characterized in that In step (2), the moisture content after drying is 4-20wt%.

7. The method according to claim 1, characterized in that The carbonization conditions include: CO2 concentration of 15-100%, temperature of 20-50°C, humidity of 40-80%, and pressurization pressure of 0-0.3MPa; and carbonization time of 6-72h.

8. The method according to claim 1, characterized in that In the obtained carbonized product, the content of aragonite is greater than 6.5 wt %, and the average particle size of aragonite is greater than 24 nm.

Citation Information

Patent Citations

  • High-magnesium low-carbon cement clinker and preparation method thereof

    CN116553842A

  • Method for desulfurizing ardealite with low carbon emission and preparing magnesium modified low-carbon clinker

    CN117700129A

Cited By

  • Lightweight carbon sequestration type cement product and preparation method thereof

    CN121872714A