Anti-corrosion metal powder reinforced concrete and preparation method thereof

By embedding nano nickel, nanochromium, and nanotitanium into low-temperature plasma ball mills, forming dense oxide films and aluminum nitride, the corrosion problem of concrete in harsh environments is solved, and the high-temperature corrosion resistance of concrete is significantly improved. Mechanical properties extend the service life of the structure.

CN119059766APending Publication Date: 2024-12-03TANGSHAN XIUXI CONSTRUCTION CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410958734.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The rust problem of concrete caused by chloride ion corrosion in harsh environments leads to damage to the durability of reinforced concrete, and expanding stress and cracks are generated inside the structure, which poses safety hazards.

Method used

Modified aluminum powder is used to embed nano nickel, nanochromium, and nanotitanium through low-temperature plasma ball mill to form a dense oxide film and aluminum nitride, enhancing the high-temperature corrosion resistance and mechanical properties of the concrete.

Benefits of technology

Effectively prevent chloride ions from erosion, improve the compressive strength and high-temperature corrosion resistance of concrete, extend the service life of the structure, and reduce safety hazards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004949667030000051
    Figure BDA0004949667030000051
Patent Text Reader

Abstract

The invention discloses anti-corrosion metal powder reinforced concrete and a preparation method thereof, and relates to the technical field of concrete. Nano nickel, nano chromium and nano titanium are embedded in an aluminum matrix through ball milling under the action of a plasma field, mechanical energy generated by ball milling acts on aluminum powder, and electron bombardment is carried out, so that errors in the matrix are proliferated, moved and creeped, a flaky body is formed, a compact oxidation film is more easily generated on the surface, and the anti-corrosion effect is achieved; the nano-nickel, the nano-chromium and the nano-titanium are embedded in the sheet-shaped body under the action of a positive force, so that high-temperature corrosion resistance is realized, then ammonia gas plasma with low discharge intensity is used for generating an electric-thermal coupling effect with aluminum ions, so that aluminum nitride is partially generated as a hard phase in a matrix and cooperates with the nano-nickel to realize relatively strong mechanical properties, and the high-temperature corrosion resistance is realized. And the high-temperature corrosion resistance is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of concrete, in particular to an anti-corrosion metal powder reinforced concrete and a preparation method thereof. Background Art

[0002] Concrete is widely used in various projects due to its economical and high strength characteristics. However, in harsh environments, due to the inherent defects of concrete materials themselves (microcracks, capillaries, etc.), its durability is seriously threatened. Among them, the corrosion of metal components caused by chloride ion erosion is one of the main factors causing the durability problem of reinforced concrete. As the service time increases, the chloride ions in the environment can be transported in the concrete through capillary adsorption and diffusion until they reach the surface of the steel bars. When the chloride ion concentration accumulates to a certain value, it will destroy the passivation film on the surface of the metal component, forming a corrosion cell and causing corrosion. The volume of the product obtained after the corrosion reaction is 2 to 6 times that before the corrosion, which will produce expansion stress in the concrete, causing cracks inside the structure and causing safety hazards. Therefore, it is particularly necessary to invent a corrosion-resistant metal powder reinforced concrete. Summary of the invention

[0003] The object of the present invention is to provide an anti-corrosion metal powder reinforced concrete and a preparation method thereof, so as to solve the problems existing in the prior art.

[0004] In order to solve the above technical problems, the present invention provides the following technical solution: an anti-corrosion metal powder reinforced concrete, wherein the anti-corrosion metal powder reinforced concrete is made of modified aluminum powder mixed concrete.

[0005] Furthermore, the modified aluminum powder is prepared by embedding nano nickel, nano chromium and nano titanium in aluminum powder through low temperature plasma ball milling.

[0006] Furthermore, a method for preparing anti-corrosion metal powder reinforced concrete comprises the following preparation steps:

[0007] (1) mixing aluminum powder, nano-nickel, nano-chromium, nano-titanium and anhydrous ethanol, and subjecting the mixture to low-temperature plasma ball milling to obtain modified aluminum powder;

[0008] (2) Modified aluminum powder, silicate cement, limestone coarse particles, limestone chips, fly ash, triterpenoid saponin, melamine, and deionized water are mixed, ultrasonically stirred, and then placed in a mold and cured for 5 to 8 hours to obtain anti-corrosion metal powder reinforced concrete.

[0009] Furthermore, the particle size of the aluminum powder in step (1) is 18 to 25 μm.

[0010] Furthermore, the process parameters of the low-temperature plasma ball milling in step (1) are as follows: the ball milling medium is a cemented carbide ball, the ball-to-material ratio is 30:1, the rotation speed is 1350 rpm, and the electric field voltage is 13-20 kV.

[0011] Furthermore, in step (1), the initial atmosphere of the low-temperature plasma milling is argon, the time is 1 to 2 hours, and the later atmosphere is ammonia, the time is 2 to 6 hours, and the gas pressure is 0.1 MPa.

[0012] Furthermore, in step (1), the mass ratio of the aluminum powder, nano-nickel, nano-chromium, nano-titanium and anhydrous ethanol is 12-22:0.3:0.3:0.3:0.6.

[0013] Furthermore, the ultrasonic frequency in step (2) is 21 to 30 kHz.

[0014] Furthermore, in step (2), the stirring rate is 100 to 200 rpm and the time is 30 to 50 min.

[0015] Furthermore, in step (2), the mass ratio of the modified aluminum powder, silicate cement, limestone coarse particles, limestone chips, fly ash, triterpenoid saponin, melamine and deionized water is 5-10:48:160:134:17:1:0.5:30.

[0016] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0017] The present invention utilizes nano nickel, nano chromium and nano titanium to be embedded in an aluminum matrix through ball milling under the action of a plasma field. When a large amount of mechanical energy generated by ball milling acts on the aluminum powder, a part of the energy causes a large number of defects to be formed inside the powder and is converted into internal energy, and the other part is released in the form of heat energy, causing the temperature inside the tank to rise. At this time, the temperature is further raised by electron bombardment, and the dislocations inside the matrix are multiplied, moved and creep, thereby continuously undergoing plastic deformation, and the micro-forging process of the powder is prolonged to form a sheet with a larger diameter and thickness, making it easier to form a dense oxide film on the surface, thereby achieving an anti-corrosion effect. In this process, nano nickel, nano chromium and nano titanium are embedded in the sheet under the action of a positive force. Under high temperature environment, titanium element can promote the formation of dense and continuous chromium oxide on the surface of the matrix, thereby achieving high temperature corrosion resistance. Then, it is replaced with ammonia plasma with low discharge intensity to induce gas-solid reaction, and produce electric-thermal coupling effect with aluminum ions, so that part of aluminum nitride is generated as a hard phase in the matrix, which cooperates with nano-nickel to achieve strong mechanical properties and further improve high temperature corrosion resistance. The presence of aluminum nitride promotes the accumulation of electric field distortion and Joule heat, which is released in the form of explosion on the surface of the matrix, leaving small molten holes, causing a large amount of stress concentration and cracks, so that larger flaky particles are broken and refined under the impact of the grinding balls, while preserving the flaky morphology, thereby improving high temperature corrosion resistance and mechanical properties. DETAILED DESCRIPTION

[0018] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0019] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the anti-corrosion metal powder reinforced concrete prepared in the following examples are as follows:

[0020] Mechanical properties: The concrete of the embodiment and the comparative example was made into specimens with a size of 100 mm×100 mm×100 mm, and the compressive strength test of the specimens at different ages was carried out with reference to GB / T50081.

[0021] High temperature resistance: Take the same size of the embodiment and the comparative example and refer to GB / T50081, burn them at 400℃ for 3h, then cool them to room temperature and test their compressive strength.

[0022] Corrosion resistance: Take the embodiment and comparative example of the same size and refer to GB / T500082 to detect the penetration depth of chloride ions.

[0023] Example 1

[0024] (1) Aluminum powder with a particle size of 18 μm, nano nickel, nano chromium, nano titanium, and anhydrous ethanol are mixed, subjected to low-temperature plasma ball milling, reacted for 1 hour in an argon environment with a gas pressure of 0.1 MPa, and then ammonia is introduced and reacted for 2 hours. The process parameters are as follows: the ball milling medium is a cemented carbide ball, the ball-to-material ratio is 30:1, the rotation speed is 1350 rpm, and the electric field voltage is 13 kV, to obtain modified aluminum powder; the mass ratio of the aluminum powder with a particle size of 18 μm, nano nickel, nano chromium, nano titanium, and anhydrous ethanol is 12:0.3:0.3:0.3:0.6;

[0025] (2) Modified aluminum powder, silicate cement, limestone coarse particles, limestone chips, fly ash, triterpenoid saponin, melamine, and deionized water are mixed, stirred at 21 kHz and 100 rpm for 30 min, then placed in a mold and cured for 5 h to obtain anti-corrosion metal powder reinforced concrete; the mass ratio of the modified aluminum powder, silicate cement, limestone coarse particles, limestone chips, fly ash, triterpenoid saponin, melamine, and deionized water is 5:48:160:134:17:1:0.5:30.

[0026] Example 2

[0027] (1) Aluminum powder with a particle size of 21 μm, nano nickel, nano chromium, nano titanium, and anhydrous ethanol are mixed, subjected to low-temperature plasma ball milling, reacted for 1.5 h in an argon environment with a gas pressure of 0.1 MPa, and then ammonia is introduced and reacted for 4 h. The process parameters are as follows: the ball milling medium is a cemented carbide ball, the ball-to-material ratio is 30:1, the rotation speed is 1350 rpm, and the electric field voltage is 16 kV, to obtain modified aluminum powder; the mass ratio of the aluminum powder with a particle size of 21 μm, nano nickel, nano chromium, nano titanium, and anhydrous ethanol is 17:0.3:0.3:0.3:0.6;

[0028] (2) Modified aluminum powder, silicate cement, limestone coarse particles, limestone chips, fly ash, triterpenoid saponin, melamine, and deionized water are mixed, stirred at 26 kHz and 150 rpm for 40 min, then placed in a mold and cured for 6 h to obtain anti-corrosion metal powder reinforced concrete; the mass ratio of the modified aluminum powder, silicate cement, limestone coarse particles, limestone chips, fly ash, triterpenoid saponin, melamine, and deionized water is 7:48:160:134:17:1:0.5:30.

[0029] Example 3

[0030] (1) Aluminum powder with a particle size of 25 μm, nano nickel, nano chromium, nano titanium, and anhydrous ethanol are mixed, subjected to low-temperature plasma ball milling, reacted for 2 h in an argon environment with a gas pressure of 0.1 MPa, and then ammonia is introduced and reacted for 6 h. The process parameters are as follows: the ball milling medium is a cemented carbide ball, the ball-to-material ratio is 30:1, the rotation speed is 1350 rpm, and the electric field voltage is 20 kV, to obtain modified aluminum powder; the mass ratio of the aluminum powder with a particle size of 25 μm, nano nickel, nano chromium, nano titanium, and anhydrous ethanol is 22:0.3:0.3:0.3:0.6;

[0031] (2) Modified aluminum powder, silicate cement, limestone coarse particles, limestone chips, fly ash, triterpenoid saponin, melamine, and deionized water are mixed, stirred at 30 kHz and 200 rpm for 50 min, then placed in a mold and cured for 8 h to obtain anti-corrosion metal powder reinforced concrete; the mass ratio of the modified aluminum powder, silicate cement, limestone coarse particles, limestone chips, fly ash, triterpenoid saponin, melamine, and deionized water is 10:48:160:134:17:1:0.5:30.

[0032] Comparative Example 1

[0033] The difference between Comparative Example 1 and Example 2 is that step (1) is different. Step (1) is changed to: aluminum powder with a particle size of 21 μm and anhydrous ethanol are mixed, subjected to low-temperature plasma ball milling, reacted for 1.5 hours in an argon environment with a gas pressure of 0.1 MPa, and then ammonia is introduced and reacted for 4 hours. The process parameters are as follows: the ball milling medium is a cemented carbide ball, the ball-to-material ratio is 30:1, the rotation speed is 1350 rpm, and the electric field voltage is 16 kV to obtain modified aluminum powder; the mass ratio of the aluminum powder with a particle size of 21 μm and anhydrous ethanol is 17:0.6; the remaining steps are the same as Example 2.

[0034] Comparative Example 2

[0035] The difference between Comparative Example 2 and Example 2 is that step (1) is different. Step (1) is changed to: aluminum powder with a particle size of 21 μm, nano nickel, nano chromium, nano titanium, and anhydrous ethanol are mixed, and low-temperature plasma ball milling is performed in an argon environment with an air pressure of 0.1 MPa. The process parameters are as follows: the ball milling medium is a cemented carbide ball, the ball-to-material ratio is 30:1, the rotation speed is 1350 rpm, the electric field voltage is 16 kV, and the time is 5.5 h to obtain modified aluminum powder; the mass ratio of the aluminum powder with a particle size of 21 μm, nano nickel, nano chromium, nano titanium, and anhydrous ethanol is 17:0.3:0.3:0.3:0.6; the remaining steps are the same as Example 2.

[0036] Comparative Example 3

[0037] The difference between Comparative Example 3 and Example 2 is that step (1) is different. Step (1) is changed to: aluminum powder with a particle size of 21 μm, nano nickel, nano chromium, nano titanium, and anhydrous ethanol are mixed, ball milled, and reacted for 1.5 hours in an argon environment with an air pressure of 0.1 MPa, and then ammonia is introduced and reacted for 4 hours. The process parameters are as follows: the ball milling medium is a cemented carbide ball, the ball-to-material ratio is 30:1, and the rotation speed is 1350 rpm to obtain modified aluminum powder; the mass ratio of the aluminum powder with a particle size of 21 μm, nano nickel, nano chromium, nano titanium, and anhydrous ethanol is 17:0.3:0.3:0.3:0.6; the remaining steps are the same as Example 2.

[0038] Effect example

[0039] Table 1 below shows the performance analysis results of the anti-corrosion metal powder reinforced concrete using Examples 1 to 3 of the present invention and Comparative Examples 1 to 3.

[0040] Table 1

[0041]

[0042] From the comparison of the experimental data of the embodiment and the comparative example in Table 1, it can be found that the present invention uses nano nickel, nano chromium, and nano titanium to be embedded in the aluminum matrix through ball milling under the action of the plasma field. When a large amount of mechanical energy generated by ball milling acts on the aluminum powder, a part of the energy causes a large number of defects to be formed inside the powder and is converted into internal energy, and the other part is released in the form of heat energy, which increases the temperature in the tank. At this time, it is bombarded by electrons, and the temperature is further increased, and the dislocations in the matrix are multiplied, moved, and creep, thereby continuously undergoing plastic deformation, and the micro-forging process of the powder is extended to form a sheet with a larger diameter and thickness, which is easier to form a dense oxide film on the surface to achieve an anti-corrosion effect. In this process, the nano nickel, nano chromium, and nano titanium are under the action of the positive force. Under high temperature environment, titanium element can promote the formation of dense and continuous chromium oxide on the surface of the matrix, thereby achieving high temperature corrosion resistance. Then, it is replaced with ammonia plasma with low discharge intensity, which induces gas-solid reaction and produces electric-thermal coupling effect with aluminum ions, so that aluminum nitride is partially generated as a hard phase in the matrix, which cooperates with nano-nickel to achieve strong mechanical properties and further improve high temperature corrosion resistance. The presence of aluminum nitride promotes the accumulation of electric field distortion and Joule heat, which is released in the form of explosion on the surface of the matrix, leaving small molten holes, thereby causing a large amount of stress concentration and generating cracks, so that larger flaky particles are broken and refined under the impact of the grinding balls, while preserving the flaky morphology, thereby improving high temperature corrosion resistance and mechanical properties.

[0043] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. An anti-corrosion metal powder reinforced concrete, characterized in that: The anti-corrosion metal powder reinforced concrete is prepared from modified aluminum powder mixed concrete.

2. The anti-corrosion metal powder reinforced concrete according to claim 1, characterized in that: The modified aluminum powder is prepared by embedding nano nickel, nano chromium and nano titanium in aluminum powder through low temperature plasma ball milling.

3. A method for preparing anti-corrosion metal powder reinforced concrete, characterized in that: The method comprises the following preparation steps: (1) mixing aluminum powder, nano-nickel, nano-chromium, nano-titanium and anhydrous ethanol, and subjecting the mixture to low-temperature plasma ball milling to obtain modified aluminum powder; (2) Modified aluminum powder, silicate cement, limestone coarse particles, limestone chips, fly ash, triterpenoid saponin, melamine, and deionized water are mixed, ultrasonically stirred, and then placed in a mold and cured for 5 to 8 hours to obtain anti-corrosion metal powder reinforced concrete.

4. The method for preparing anti-corrosion metal powder reinforced concrete according to claim 3, characterized in that: The particle size of the aluminum powder in step (1) is 18 to 25 μm.

5. The method for preparing anti-corrosion metal powder reinforced concrete according to claim 3, characterized in that: The process parameters of the low-temperature plasma ball milling in step (1) are as follows: the ball milling medium is a cemented carbide ball, the ball-to-material ratio is 30:1, the rotation speed is 1350 rpm, and the electric field voltage is 13-20 kV.

6. The method for preparing anti-corrosion metal powder reinforced concrete according to claim 3, characterized in that: In step (1), the low-temperature plasma milling is performed in an initial atmosphere of argon for 1 to 2 hours, and in a later atmosphere of ammonia for 2 to 6 hours, with an air pressure of 0.1 MPa.

7. The method for preparing anti-corrosion metal powder reinforced concrete according to claim 3, characterized in that: The mass ratio of the aluminum powder, nano-nickel, nano-chromium, nano-titanium and anhydrous ethanol in step (1) is 12-22:0.3:0.3:0.3:0.

6.

8. The method for preparing anti-corrosion metal powder reinforced concrete according to claim 3, characterized in that: The ultrasonic frequency in step (2) is 21 to 30 kHz.

9. The method for preparing anti-corrosion metal powder reinforced concrete according to claim 3, characterized in that: The stirring rate of step (2) is 100-200 rpm and the time is 30-50 min.

10. The method for preparing anti-corrosion metal powder reinforced concrete according to claim 3, characterized in that: The mass ratio of the modified aluminum powder, silicate cement, limestone coarse particles, limestone chips, fly ash, triterpenoid saponin, melamine and deionized water in step (2) is 5-10:48:160:134:17:1:0.5:30.