Carbonized recycled aggregate high-strength pervious concrete and preparation method thereof
Carbonizing recycled aggregates and integrating them into a specific concrete mix enhances the strength and permeability of permeable concrete, addressing the challenges of recycled aggregate use and promoting resource recycling.
Patent Information
- Application Number
- CN202411020391.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-07-29
AI Technical Summary
Existing permeable concrete technologies face challenges in enhancing strength while maintaining permeability, leading to increased construction costs and difficulties, particularly when using recycled aggregates.
A carbonized recycled aggregate high-strength permeable concrete is prepared using a method that includes carbonizing recycled concrete aggregates under specific conditions and incorporating them in a high proportion with cement, fly ash, silica fume, river sand, and water reducer to form a high-strength permeable concrete.
The method effectively improves the mechanical properties and permeability of permeable concrete, allowing for large-scale resource recycling and reducing carbon emissions, while ensuring strength and permeability requirements are met.
Smart Images

Figure CN119059767A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of construction solid waste recycling, and in particular to a recycled aggregate high-strength permeable concrete and a preparation method and application thereof. Background Art
[0002] Permeable concrete is also called porous concrete and sandless concrete. It is a porous lightweight concrete made of aggregate (stone), cement, reinforcing agent, and water in a certain ratio. Permeable concrete is a honeycomb structure with uniformly distributed pores formed by a thin layer of cement slurry coated on the surface of coarse aggregate, which is bonded to each other. Therefore, it has the characteristics of air permeability, water permeability and light weight. At the same time, permeable concrete pavement is a green building material that can reduce the heat island effect, absorb road noise, promote rainwater runoff and purify water quality. Therefore, permeable concrete pavement, as a rainwater management device, can effectively control urban rainwater runoff. It has become a permeable product that is given priority in urban construction.
[0003] At present, one of the challenges in the road construction industry is to improve the strength of permeable bricks. In order to break through this bottleneck, researchers have improved the strength of permeable concrete by adding polyacrylamide to adjust the film-forming ability, adding steel fibers and applying slurry on the surface to strengthen aggregates. However, since permeable concrete itself is a porous system, how to prepare permeable concrete by strengthening aggregates with cement paste and at the same time, ensuring the permeability of permeable concrete has become a difficult problem. However, this will not only increase the construction cost and difficulty, but also increase large-scale applications in the road construction industry. Summary of the invention
[0004] The present invention provides a carbonized recycled aggregate high-strength permeable concrete and a preparation method thereof, which effectively solves the technical difficulty of low strength of permeable concrete due to recycled aggregate, promotes the application of recycled concrete aggregate in the preparation of permeable concrete, and expands the resource utilization of carbonization technology. To achieve the above purpose, the technical solution of the present invention is as follows.
[0005] The present invention provides a carbonized recycled aggregate high-strength permeable concrete, comprising raw materials:
[0006] 300-500 parts by weight of cement, 100-200 parts by weight of fly ash, 80-150 parts by weight of silica fume, 400-600 parts by weight of river sand, 1500-2500 parts by weight of the aggregate, 20-40 parts by weight of water reducer and 100-200 parts by weight of mixing water, wherein the aggregate comprises carbonized recycled concrete aggregate.
[0007] Furthermore, the carbonized recycled concrete aggregate content is not less than 50% of the aggregate.
[0008] Furthermore, the method for preparing carbonized recycled concrete aggregate comprises:
[0009] The recycled aggregate is placed in a pressure tank: the recycled aggregate is carbonized under the conditions of 0.1 MPa pressure, 25° C. temperature, 70% humidity, and 99% carbon dioxide concentration to obtain carbonized recycled concrete aggregate.
[0010] Furthermore, the particle size of the recycled aggregate is 2 to 10 mm.
[0011] Furthermore, the particle size of the river sand is 0.5 mm to 1.18 mm.
[0012] Furthermore, the ratio of the mixing water to the water reducing agent ranges from 0.18 to 0.20.
[0013] Furthermore, the cement is ordinary Portland cement.
[0014] Furthermore, the recycled aggregate is prepared from urban abandoned road aggregate.
[0015] Another aspect of the present invention further discloses a method for preparing the carbonized recycled aggregate high-strength permeable concrete, comprising:
[0016] Step 1: crushing urban abandoned road aggregate to obtain recycled aggregate, and then sieving to obtain recycled concrete aggregate with a specified particle size; after completion, separating the aggregate to obtain pre-treated recycled aggregate;
[0017] Step 2: Put the recycled aggregate into a pressure tank for carbonization to obtain carbonized recycled concrete aggregate.
[0018] Step 3: Mix the raw materials evenly and stir for the prescribed time, then press and form to obtain permeable concrete.
[0019] Furthermore, the method further comprises step 4: the permeable concrete is cured at room temperature for 28 days to obtain carbonized recycled aggregate high-strength permeable concrete.
[0020] Compared with the prior art, the present invention effectively solves the problem of poor stress-bearing performance of recycled aggregates, effectively improves the recycled aggregates by carbonization, broadens the application scenarios of high-strength permeable concrete with carbonized recycled aggregates, provides a solution for alleviating carbon emissions, and promotes large-scale resource recycling of urban construction solid waste. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 These are the samples of carbonized recycled concrete aggregate of Examples 1-4 and Comparative Examples 1-4.
[0022] Figure 2 Schematic diagram of pressurized forming of permeable concrete.
[0023] Figure 3The present invention is a flow chart of the process for preparing high-strength permeable concrete with carbonized recycled aggregate. DETAILED DESCRIPTION
[0024] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only embodiments of a part of the present invention, rather than all embodiments.
[0025] The technical solutions in the embodiments of the present invention will be described clearly and completely below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the implementation cases in the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] The embodiment of the present invention provides a carbonized recycled aggregate high-strength permeable concrete, including raw materials:
[0027] 300-500 parts by weight of cement, 100-200 parts by weight of fly ash, 80-150 parts by weight of silica fume, 400-600 parts by weight of river sand, 1500-2500 parts by weight of the aggregate, 20-40 parts by weight of water reducer and 100-200 parts by weight of mixing water, wherein the aggregate comprises carbonized recycled concrete aggregate.
[0028] Optionally, the carbonized recycled concrete aggregate content is not less than 50% of the aggregate.
[0029] Optionally, the method for preparing carbonized recycled concrete aggregate comprises:
[0030] The recycled aggregate is placed in a pressure tank: the recycled aggregate is carbonized under the conditions of 0.1 MPa pressure, 25° C. temperature, 70% humidity, and 99% carbon dioxide concentration to obtain carbonized recycled concrete aggregate.
[0031] Particularly, the particle size of the recycled aggregate is 2 to 10 mm.
[0032] Optionally, the particle size of the river sand is 0.5 mm to 1.18 mm.
[0033] Optionally, the ratio of mixing water to water reducing agent ranges from 0.18 to 0.20.
[0034] Optionally, the cement is ordinary Portland cement.
[0035] Particularly, the recycled aggregate is prepared from urban abandoned road aggregate.
[0036] The present invention also provides a method for preparing high-performance carbonized recycled aggregate high-strength permeable concrete, comprising:
[0037] Add cement, fly ash, silica fume, sand and water reducing agent into the mixer at a slow speed for 3 minutes and at a fast speed for 3 minutes;
[0038] Add recycled aggregate and continue stirring for 3 minutes;
[0039] The molding mold for the mixture is made of steel and is pressed and molded using a press with a load of 1Mpa. The mixture must be spread twice and compacted once.
[0040] To further illustrate the embodiments of the present invention and their effects, embodiments 1-4 are listed below.
[0041] Example 1
[0042] A carbonized recycled aggregate high-strength permeable concrete and a preparation method thereof, comprising the following steps:
[0043] (1) crushing urban abandoned road aggregate to obtain recycled aggregate, and then using screening to obtain recycled concrete aggregate with an aggregate particle size of 2.36-5 mm; after completion, separating the aggregate to obtain pre-treated recycled concrete aggregate;
[0044] (2) The pretreated recycled concrete aggregate was placed in a pressure tank: the pretreated recycled concrete aggregate was carbonized for 24 hours under the conditions of a pressure of 0.1 MPa, a temperature of 25° C., a humidity of 70%, and a carbon dioxide concentration of 99% to obtain a carbonized recycled concrete aggregate.
[0045] (3) 404 parts by weight of cement, 173 parts by weight of fly ash, 110 parts by weight of silica fume, 531 parts by weight of river sand, 870 parts by weight of pretreated recycled concrete aggregate, 870 parts by weight of carbonized recycled concrete aggregate, 27 parts by weight of water reducer and 123 parts by weight of mixing water were uniformly mixed for a prescribed stirring time and pressurized to obtain permeable concrete.
[0046] The permeable concrete of this embodiment was prepared into a test specimen and cured in a water curing box for 28 days. The compressive strength of the specimen was then tested according to the Technical Specification for Application of Carbonized Recycled Aggregate High-Strength Permeable Concrete (CJJT-253-2016), and the test result was 28.02 MPa.
[0047] Example 2
[0048] A carbonized recycled aggregate high-strength permeable concrete and a preparation method thereof, comprising the following steps:
[0049] (1) crushing urban abandoned road aggregate to obtain recycled aggregate, and then using screening to obtain recycled concrete aggregate with an aggregate particle size of 2.36-5 mm; after completion, separating the aggregate to obtain pre-treated recycled concrete aggregate;
[0050] (2) The pretreated recycled concrete aggregate was placed in a pressure tank: the pretreated recycled concrete aggregate was carbonized for 24 hours under the conditions of a pressure of 0.1 MPa, a temperature of 25° C., a humidity of 70%, and a carbon dioxide concentration of 99% to obtain a carbonized recycled concrete aggregate.
[0051] (3) 404 parts by weight of cement, 173 parts by weight of fly ash, 110 parts by weight of silica fume, 531 parts by weight of river sand, 1740 parts by weight of the carbonized recycled concrete aggregate, 27 parts by weight of water reducer and 123 parts by weight of mixing water were uniformly mixed for a prescribed stirring time and pressurized to obtain permeable concrete.
[0052] The permeable concrete of this embodiment was prepared into a test specimen and cured in a water curing box for 28 days. The compressive strength of the specimen was then tested according to the Technical Specification for Application of Carbonized Recycled Aggregate High-Strength Permeable Concrete (CJJT-253-2016), and the test result was 32.74 MPa.
[0053] Example 3
[0054] A carbonized recycled aggregate high-strength permeable concrete and a preparation method thereof, comprising the following steps:
[0055] (1) crushing urban abandoned road aggregate to obtain recycled aggregate, and then using screening to obtain recycled concrete aggregate with an aggregate particle size of 5-10 mm; after completion, separating the aggregate to obtain pre-treated recycled concrete aggregate;
[0056] (2) The pretreated recycled concrete aggregate was placed in a pressure tank: the pretreated recycled concrete aggregate was carbonized for 24 hours under the conditions of a pressure of 0.1 MPa, a temperature of 25° C., a humidity of 70%, and a carbon dioxide concentration of 99% to obtain a carbonized recycled concrete aggregate.
[0057] (3) 404 parts by weight of cement, 173 parts by weight of fly ash, 110 parts by weight of silica fume, 531 parts by weight of river sand, 1111 parts by weight of pretreated recycled concrete aggregate, 1111 parts by weight of carbonized recycled concrete aggregate, 27 parts by weight of water reducer and 123 parts by weight of mixing water were uniformly mixed for a prescribed stirring time and pressurized to obtain permeable concrete.
[0058] The permeable concrete of this embodiment was prepared into a test specimen and cured in a water curing box for 28 days. The compressive strength of the specimen was then tested according to the Technical Specification for Application of Carbonized Recycled Aggregate High-Strength Permeable Concrete (CJJT-253-2016), and the test result was 25.49 MPa.
[0059] Example 4
[0060] A carbonized recycled aggregate high-strength permeable concrete and a preparation method thereof, comprising the following steps:
[0061] (1) crushing urban abandoned road aggregate to obtain recycled aggregate, and then using screening to obtain recycled concrete aggregate with an aggregate particle size of 5-10 mm; after completion, separating the aggregate to obtain pre-treated recycled concrete aggregate;
[0062] (2) The pretreated recycled concrete aggregate was placed in a pressure tank: the pretreated recycled concrete aggregate was carbonized for 24 hours under the conditions of a pressure of 0.1 MPa, a temperature of 25° C., a humidity of 70%, and a carbon dioxide concentration of 99% to obtain a carbonized recycled concrete aggregate.
[0063] (3) 404 parts by weight of cement, 173 parts by weight of fly ash, 110 parts by weight of silica fume, 531 parts by weight of river sand, 2065 parts by weight of carbonized recycled concrete aggregate, 27 parts by weight of water reducer and 123 parts by weight of mixing water were uniformly mixed for a prescribed stirring time and pressurized to obtain permeable concrete.
[0064] The permeable concrete of this embodiment was prepared into a test specimen and cured in a water curing box for 28 days. The compressive strength of the specimen was then tested according to the Technical Specification for Application of Carbonized Recycled Aggregate High-Strength Permeable Concrete (CJJT-253-2016), and the test result was 28.81 MPa.
[0065] Comparative Example 1
[0066] The concrete preparation of Comparative Example 1 includes the following steps:
[0067] (1) crushing natural aggregate to obtain aggregate, and then sieving to obtain natural aggregate with an aggregate particle size of 2.36-5 mm; after completion, separating the aggregate to obtain pretreated aggregate;
[0068] (2) The natural aggregate is placed under normal temperature and pressure and directly used for the test.
[0069] (3) 404 parts by weight of cement, 173 parts by weight of fly ash, 110 parts by weight of silica fume, 531 parts by weight of river sand, 1740 parts by weight of the reconcrete aggregate, 27 parts by weight of water reducer and 123 parts by weight of mixing water are uniformly mixed for a prescribed stirring time and pressure-formed to obtain permeable concrete.
[0070] The permeable concrete of this embodiment was prepared into a test specimen and cured in a water curing box for 28 days. The compressive strength of the specimen was then tested according to the Technical Specification for Application of Carbonized Recycled Aggregate High-Strength Permeable Concrete (CJJT-253-2016), and the test result was 45.59 MPa.
[0071] Comparative Example 2
[0072] The concrete preparation of Comparative Example 2 includes the following steps:
[0073] (1) crushing natural aggregate to obtain aggregate, and then using screening to obtain natural aggregate with an aggregate particle size of 5-10 mm; after completion, separating the aggregate to obtain pretreated aggregate;
[0074] (2) The natural aggregate is placed under normal temperature and pressure and directly used for the test.
[0075] (3) 404 parts by weight of cement, 173 parts by weight of fly ash, 110 parts by weight of silica fume, 531 parts by weight of river sand, 2065 parts by weight of the natural aggregate, 27 parts by weight of water reducer and 123 parts by weight of mixing water are uniformly mixed for a prescribed stirring time and pressure-formed to obtain permeable concrete.
[0076] The permeable concrete of this embodiment was prepared into a test specimen and cured in a water curing box for 28 days. The compressive strength of the specimen was then tested according to the Technical Specification for Application of Carbonized Recycled Aggregate High-Strength Permeable Concrete (CJJT-253-2016), and the test result was 37.17 MPa.
[0077] Comparative Example 3
[0078] The concrete preparation of Comparative Example 3 includes the following steps:
[0079] (1) crushing urban abandoned road aggregate to obtain recycled aggregate, and then using screening to obtain recycled concrete aggregate with an aggregate particle size of 2.36-5 mm; after completion, separating the aggregate to obtain pre-treated recycled concrete aggregate;
[0080] (2) 404 parts by weight of cement, 173 parts by weight of fly ash, 110 parts by weight of silica fume, 531 parts by weight of river sand, 1740 parts by weight of pretreated recycled concrete aggregate, 27 parts by weight of water reducer and 123 parts by weight of mixing water were uniformly mixed for a prescribed stirring time and pressurized to obtain permeable concrete.
[0081] The permeable concrete of this embodiment was prepared into a test specimen and cured in a water curing box for 28 days. The compressive strength of the specimen was then tested according to the Technical Specification for Application of Carbonized Recycled Aggregate High-Strength Permeable Concrete (CJJT-253-2016), and the test result was 26.92 MPa.
[0082] Comparative Example 4
[0083] The concrete preparation of Comparative Example 4 includes the following steps:
[0084] (1) crushing urban abandoned road aggregate to obtain recycled aggregate, and then using screening to obtain recycled concrete aggregate with an aggregate particle size of 5-10 mm; after completion, separating the aggregate to obtain pre-treated recycled concrete aggregate;
[0085] (2) 404 parts by weight of cement, 173 parts by weight of fly ash, 110 parts by weight of silica fume, 531 parts by weight of river sand, 2065 parts by weight of pretreated recycled concrete aggregate, 27 parts by weight of water reducer and 123 parts by weight of mixing water were uniformly mixed for a prescribed stirring time and pressurized to obtain permeable concrete.
[0086] The permeable concrete of this embodiment was prepared into a test specimen and cured in a water curing box for 28 days. The compressive strength of the specimen was then tested according to the Technical Specification for Application of Carbonized Recycled Aggregate High-Strength Permeable Concrete (CJJT-253-2016), and the test result was 24.98 MPa.
[0087] Comparative Example 5
[0088] The concrete preparation of Comparative Example 5 includes the following steps:
[0089] (1) crushing urban abandoned road aggregate to obtain recycled aggregate, and then using screening to obtain recycled concrete aggregate with an aggregate particle size of 2.36-5 mm; after completion, separating the aggregate to obtain pre-treated recycled concrete aggregate;
[0090] (2) The pretreated recycled concrete aggregate was placed in a pressure tank: the pretreated recycled concrete aggregate was carbonized for 24 hours under the conditions of a pressure of 0.1 MPa, a temperature of 25° C., a humidity of 70%, and a carbon dioxide concentration of 99% to obtain a carbonized recycled concrete aggregate.
[0091] (3) 404 parts by weight of cement, 173 parts by weight of fly ash, 110 parts by weight of silica fume, 531 parts by weight of river sand, 1740 parts by weight of carbonized recycled concrete aggregate, 27 parts by weight of water reducer and 123 parts by weight of mixing water were uniformly mixed for a prescribed stirring time without being pressed to obtain permeable concrete.
[0092] The permeable concrete of this embodiment was prepared into a test specimen and cured in a water curing box for 28 days. The compressive strength of the specimen was then tested according to the Technical Specification for Application of Recycled Aggregate Permeable Concrete (CJJT-253-2016), and the test result was 29.83 MPa.
[0093] Comparative Example 6
[0094] The concrete preparation of Comparative Example 6 includes the following steps:
[0095] (1) crushing urban abandoned road aggregate to obtain recycled aggregate, and then using screening to obtain recycled concrete aggregate with an aggregate particle size of 5-10 mm; after completion, separating the aggregate to obtain pre-treated recycled concrete aggregate;
[0096] (2) The pretreated recycled concrete aggregate was placed in a pressure tank: the pretreated recycled concrete aggregate was carbonized for 24 hours under the conditions of a pressure of 0.1 MPa, a temperature of 25° C., a humidity of 70%, and a carbon dioxide concentration of 99% to obtain a carbonized recycled concrete aggregate.
[0097] (3) 404 parts by weight of cement, 173 parts by weight of fly ash, 110 parts by weight of silica fume, 531 parts by weight of river sand, 2065 parts by weight of carbonized recycled concrete aggregate, 27 parts by weight of water reducer and 123 parts by weight of mixing water were uniformly mixed for a prescribed stirring time without pressure forming to obtain permeable concrete.
[0098] The permeable concrete of this embodiment was prepared into a test specimen and cured in a water curing box for 28 days. The compressive strength of the specimen was then tested according to the Technical Specification for Application of Recycled Aggregate Permeable Concrete (CJJT-253-2016), and the test result was 25.59 MPa.
[0099] Performance Testing
[0100] After curing for 28 days, the concrete of Examples 1-4 and Comparative Examples 1-4 were subjected to compressive strength, density, water permeability coefficient and effective porosity tests of permeable concrete, with reference to "CJJT-253-2016 Technical Specification for Application of Carbonized Recycled Aggregate High-Strength Permeable Concrete"; the test results are shown in the following table:
[0101] Physical and mechanical properties of high-strength permeable concrete with carbonized recycled aggregate
[0102]
[0103] Comparing the test results of Examples 1-4 with those of Comparative Examples 1-4, it can be seen that the results show that the particle size performance of carbonized fine aggregate is better than the mechanical properties of carbonized coarse aggregate; as the replacement rate of carbonized recycled aggregate increases, the performance of permeable concrete improves; when the content of carbonized recycled aggregate is 100%, the 28d compressive strength of permeable concrete prepared with aggregate particle sizes of 2.36-5mm and 5-10mm is increased by 21.62% and 15.32% respectively, the mechanical properties are effectively improved, and the permeability coefficient can still be guaranteed to meet the requirements of the specification.
[0104] In addition, the carbonization of recycled concrete aggregates can effectively fix carbon, as shown in the following table.
[0105]
[0106] In summary, the design method of high-performance carbonized recycled aggregate high-strength permeable concrete provided by the present invention has the following beneficial effects:
[0107] 1. The permeable concrete of the present invention uses construction waste aggregate as raw material, which is used as aggregate for permeable concrete after carbonization treatment, thereby alleviating the problem of deterioration of the strength of permeable concrete caused by recycled aggregate.
[0108] 2. According to the use of different road application scenarios, based on the high-performance cement-based materials with low water-cement ratio, by adding recycled concrete aggregates in high proportion, the four groups of embodiments significantly improved the mechanical properties and water permeability of the carbonized recycled aggregate high-strength permeable concrete to meet the application requirements, and the volume stability performance was guaranteed. At the same time, the four groups of embodiments and the six groups of comparative examples reflected that the performance of fine aggregate was stronger than that of coarse aggregate, and the pressurization scheme of the embodiments of the present invention could effectively improve the compressive strength of concrete;
[0109] 3. Through the mix design of carbonized recycled aggregate high-strength permeable concrete, the influence of high-performance cement matrix and recycled aggregate content on the mechanical properties and volume stability of permeable concrete can be analyzed, so as to prepare a carbonized recycled aggregate high-strength permeable concrete with comprehensive mechanical properties, permeability and volume stability;
[0110] 4. The present invention broadens the application scenarios of high-strength permeable concrete made of carbonized recycled aggregate, provides a solution for alleviating carbon emissions, and promotes large-scale resource recycling of urban construction solid waste.
[0111] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that after reading the specification of this application, the technicians can still modify or replace the specific implementation mode of the present invention with equivalents, but these modifications or changes do not deviate from the scope of protection of the pending claims of the present application.
Claims
1. A carbonized recycled aggregate high-strength permeable concrete, characterized in that: The carbonized recycled aggregate high-strength permeable concrete comprises the following raw materials: 300-500 parts by weight of cement, 100-200 parts by weight of fly ash, 80-150 parts by weight of silica fume, 400-600 parts by weight of river sand, 1500-2500 parts by weight of the aggregate, 20-40 parts by weight of water reducer and 100-200 parts by weight of mixing water, wherein the aggregate comprises carbonized recycled concrete aggregate.
2. The carbonized recycled aggregate high-strength permeable concrete according to claim 1, characterized in that: The carbonized recycled concrete aggregate content is not less than 50% of the aggregate.
3. The carbonized recycled aggregate high-strength permeable concrete according to claim 1, characterized in that: The method for preparing carbonized recycled concrete aggregate comprises: The recycled aggregate is placed in a pressure tank: the recycled aggregate is carbonized under the conditions of 0.1 MPa pressure, 25° C. temperature, 70% humidity, and 99% carbon dioxide concentration to obtain carbonized recycled concrete aggregate.
4. The carbonized recycled aggregate high-strength permeable concrete according to claim 3, characterized in that: The particle size of the recycled aggregate is 2 to 10 mm.
5. The carbonized recycled aggregate high-strength permeable concrete according to claim 1, characterized in that: The particle size of the river sand is 0.5 mm to 1.18 mm.
6. The carbonized recycled aggregate high-strength permeable concrete according to claim 1, characterized in that: The ratio of mixing water to water reducing agent ranges from 0.18 to 0.
20.
7. The carbonized recycled aggregate high-strength permeable concrete according to claim 1, characterized in that: The cement is ordinary Portland cement.
8. The carbonized recycled aggregate high-strength permeable concrete according to claim 3, characterized in that: The recycled aggregate is prepared from urban abandoned road aggregate.
9. A method for preparing the carbonized recycled aggregate high-strength permeable concrete according to any one of claims 1 to 8, characterized in that: include: Step 1: crushing urban abandoned road aggregate to obtain recycled aggregate, and then sieving to obtain recycled concrete aggregate with a specified particle size; after completion, separating the aggregate to obtain pre-treated recycled aggregate; Step 2: Put the recycled aggregate into a pressure tank for carbonization to obtain carbonized recycled concrete aggregate. Step 3: Mix the raw materials evenly and stir for the prescribed time, then press and form to obtain permeable concrete.
10. The preparation method according to claim 9, characterized in that: The method also includes step 4: the permeable concrete is cured at room temperature for 28 days to obtain carbonized recycled aggregate high-strength permeable concrete.
Citation Information
Patent Citations
Porous cement concrete using regenerative concrete aggregate
CN101407390A
Mixed admixture modified permeable recycled concrete and preparation method thereof
CN112919865A
Design method of high-performance recycled aggregate pervious concrete
CN114580200A
High-performance concrete and preparation method thereof
CN117756479A