Impermeable recycled concrete and preparation method thereof

Through specific raw material ratios and process treatment, the compressive strength and permeability of recycled concrete are improved, the problem of insufficient recycled concrete performance is solved, and efficient resource recycling and environmentally friendly concrete preparation are achieved.

CN119059768APending Publication Date: 2024-12-03WUHAN ZHONGYANGMING BUILDING MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411096494.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The compressive strength and permeability of existing recycled concrete are generally lower than those of concrete prepared with natural aggregates. It is mainly due to the cracks and pores of recycled aggregates, which affects the hydration process and interface adhesion, and increases corrosion. and risk of freeze-thaw damage.

Method used

Specific raw material ratios are adopted, including cement, regenerated coarse aggregate, regenerated fine aggregate, mineral blend, polycarboxylic acid high-performance water reducer, stannous chloride, glycol butyl ether acetate and stearic acid Magnesium intercalated hydrotalcite improves compactness through mineral blends, polycarboxylic acid water reducing agent reduces water consumption, and magnesium stearate intercalated hydrotalcite blocks moisture and ion penetration, improving permeability and compressive strength.

Benefits of technology

The resulting permeability recycled concrete has good permeability and high compressive strength, which reduces resource consumption and waste emissions, improves the density and durability of concrete, and reduces porosity and corrosion risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004988081660000061
    Figure BDA0004988081660000061
  • Figure BDA0004988081660000071
    Figure BDA0004988081660000071
Patent Text Reader

Abstract

The invention relates to the technical field of concrete. The invention discloses impermeable recycled concrete and a preparation method thereof. The impermeable recycled concrete is prepared from the following raw materials: cement, recycled coarse aggregate, recycled fine aggregate, a mineral admixture, a polycarboxylic acid high-performance water reducing agent, stannous chloride, ethylene glycol butyl ether acetate, magnesium stearate intercalated hydrotalcite and water. The preparation method comprises the following steps: S1, mixing and stirring the polycarboxylic acid high-performance water reducing agent, stannous chloride, ethylene glycol butyl ether acetate and magnesium stearate intercalated hydrotalcite to prepare a premix; s2, mixing and stirring the recycled coarse aggregate, the recycled fine aggregate and the mineral admixture, adding the premix, and stirring to obtain a mixture; and S3, adding cement and water into the mixture, stirring, injecting into a mold for molding, curing, and demolding to obtain the anti-permeability recycled concrete. The impermeable recycled concrete prepared by the invention is good in impermeability and high in compressive strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of concrete technology, and in particular to an anti-seepage recycled concrete and a preparation method thereof. Background Art

[0002] With the acceleration of urbanization and the continuous renewal of infrastructure, the construction industry has generated a large amount of waste, of which waste concrete accounts for a large proportion. The treatment of waste concrete has also become an important issue for environmental protection and sustainable development. Traditionally, waste concrete is mostly landfilled as construction waste. Although this treatment method is simple and low-cost, in the long run, it not only occupies land resources, but also poses a potential risk of pollution to soil and groundwater.

[0003] In order to reduce the impact on the environment and realize the recycling of resources, the concept of recycled aggregate has been proposed and gradually applied to the concrete industry. Recycled aggregate refers to the aggregate obtained after a series of processing processes such as crushing and screening of waste concrete, which is used to replace part or all of the natural aggregate to prepare recycled concrete. This method can theoretically reduce the cost of new concrete, reduce the exploitation of natural resources, and promote the recycling of waste. The cost and technical requirements are relatively low, and it has high promotion potential and value.

[0004] However, concrete made from recycled aggregates has obvious limitations in performance. The compressive strength and impermeability of recycled concrete are generally lower than those of concrete made from natural aggregates. This is mainly because the recycled aggregates themselves have more cracks and pores, which lead to a higher water absorption rate. When used in concrete, they will excessively absorb water from the cement paste, affecting the hydration process of the cement, resulting in insufficient hydration of the cement material and failure to generate sufficient hydration products, thereby weakening the interfacial bonding between the recycled aggregate and the cement matrix, making the concrete prone to cracking when subjected to load. In addition, these cracks and pores also provide penetration paths for corrosive media such as water and chloride ions, reducing the concrete's impermeability and increasing the risk of corrosion of steel bars in the concrete and freeze-thaw damage to the concrete.

[0005] Therefore, there is an urgent need to develop a recycled concrete with good impermeability and high compressive strength. Summary of the invention

[0006] In order to solve at least one of the above technical problems and develop a recycled concrete with good impermeability and high compressive strength, the present application provides an impermeable recycled concrete and a preparation method thereof.

[0007] On the one hand, the present application provides an impermeable recycled concrete, whose raw material composition includes, by weight: 180-220 parts of cement, 400-600 parts of recycled coarse aggregate, 200-300 parts of recycled fine aggregate, 100-150 parts of mineral admixture, 1-3 parts of polycarboxylic acid high-performance water reducer, 0.1-0.5 parts of stannous chloride, 0.5-2 parts of ethylene glycol butyl ether acetate, 1-5 parts of magnesium stearate intercalated hydrotalcite, and 150-170 parts of water.

[0008] By adopting the above technical scheme, the present application adopts specific raw materials and proportions to obtain impermeable recycled concrete with good impermeability and high compressive strength. The present application uses recycled aggregates to replace natural aggregates, which helps to reduce resource consumption and waste emissions. Mineral admixtures can improve the working performance of concrete, increase density, improve impermeability and compressive strength, and can also participate in secondary hydration reactions to generate more hydration products, fill pores, and improve the density of concrete. Polycarboxylic acid high-performance water reducer can greatly reduce the water consumption of concrete, improve fluidity while increasing the strength of concrete, reduce pores, and improve impermeability. The present application also adds stannous chloride, which can improve the durability of concrete; ethylene glycol butyl ether acetate can improve the dispersibility and stability of cement slurry and improve the performance of concrete.

[0009] The present invention adds magnesium stearate intercalated hydrotalcite, whose layered structure can block the penetration of water molecules and corrosive ions, thereby improving the impermeability and durability of concrete, and can also improve the compressive strength of concrete.

[0010] Optionally, the raw material composition includes, by weight: 190-210 parts of cement, 450-550 parts of recycled coarse aggregate, 220-280 parts of recycled fine aggregate, 110-140 parts of mineral admixture, 1.5-2.5 parts of polycarboxylic acid high-performance water reducer, 0.2-0.4 parts of stannous chloride, 1-1.5 parts of ethylene glycol butyl ether acetate, 2-4 parts of magnesium stearate intercalated hydrotalcite, and 155-165 parts of water.

[0011] Optionally, the raw material composition includes, by weight: 200 parts of cement, 500 parts of recycled coarse aggregate, 250 parts of recycled fine aggregate, 125 parts of mineral admixture, 2 parts of polycarboxylic acid high-performance water reducer, 0.3 parts of stannous chloride, 1.3 parts of ethylene glycol butyl ether acetate, 3 parts of magnesium stearate intercalated hydrotalcite, and 160 parts of water.

[0012] Optionally, the recycled coarse aggregate is composed of secondary particle sizes of 5-10 mm and 16-25 mm, and the blending ratio is 1:1.5-3.

[0013] By adopting the above technical solution, the grading and blending ratio of the recycled coarse aggregate in the present application can form a tighter aggregate arrangement, thereby improving the density of the concrete, reducing internal pores, and improving the impermeability and compressive strength of the concrete.

[0014] Optionally, the average particle size of the recycled fine aggregate is 2 to 3.5 mm.

[0015] By adopting the above technical solution, the average particle size of the recycled fine aggregate of the present application helps to improve the fluidity of concrete, making it easier for the concrete to flow and fill every corner of the formwork, thereby reducing the pores inside the concrete and improving the density.

[0016] Optionally, the mineral admixture includes ultrafine slag powder and fly ash, and the weight ratio of the ultrafine slag powder to fly ash is 2 to 3:1.

[0017] By adopting the above technical solution, ultrafine slag powder is an active mineral admixture that can react with calcium hydroxide produced by cement hydration to generate hydrated calcium silicate and hydrated calcium aluminate. These products can fill the pores of concrete, improve the density of concrete, and thus enhance its compressive strength and durability. Fly ash is also active and can improve the working performance of concrete, reduce the amount of cement, and participate in secondary hydration reactions. The generated hydration products help improve the impermeability and erosion resistance of concrete. The appropriate weight ratio helps to improve the strength of concrete.

[0018] Optionally, the specific surface area of ​​the ultrafine slag powder is not less than 700m 2 / kg, loss on ignition is not more than 1.6%.

[0019] By adopting the above technical solution, the ultra-fine slag powder with high specific surface area can react with calcium hydroxide in cement faster to generate more cementitious products such as hydrated calcium silicate, thereby significantly improving the early and late strength of concrete, while improving the density and impermeability of concrete. The smaller the loss on ignition, the lower the proportion of inactive components in the slag powder, the more active components, and therefore the better the performance of the concrete.

[0020] Optionally, the preparation method of the magnesium stearate intercalated hydrotalcite is: Step 1: Mix Mg(NO3)2·6H2O and Al(NO3)3·9H2O, add water to dissolve, and prepare a mixed salt solution; Mg 2+ and Al 3+ The molar ratio is 2 to 3:1; Step 2: adding a sodium hydroxide solution dropwise to the mixed salt solution, stirring to generate a precipitate, filtering, washing, and drying to obtain a basic hydrotalcite; Step 3: dissolving magnesium stearate in water to prepare a magnesium stearate solution; Step 4: adding the base hydrotalcite to the magnesium stearate solution, stirring at 80-90° C. for 4-20 hours, filtering, washing, and drying to obtain magnesium stearate intercalated hydrotalcite.

[0021] Optionally, the weight ratio of the stannous chloride to the magnesium stearate intercalated hydrotalcite is 1:8-12.

[0022] By adopting the above technical solution, stannous chloride and magnesium stearate intercalated hydrotalcite work together to improve the microstructure formed during cement hydration, reduce porosity, and thus improve the impermeability and compressive strength of concrete.

[0023] In a second aspect, the present application provides a method for preparing the above-mentioned impermeable recycled concrete, comprising the following steps: S1, mixing the polycarboxylic acid high-performance water-reducing agent, stannous chloride, ethylene glycol butyl ether acetate and magnesium stearate intercalated hydrotalcite, stirring to prepare a premix; S2, mixing the recycled coarse aggregate, recycled fine aggregate and mineral admixture, stirring, adding the premix, stirring, and obtaining a mixture; S3, adding cement and water to the mixture, stirring, injecting into a mold for molding, curing, and demoulding to obtain impermeable recycled concrete.

[0024] By adopting the above technical solution, the preparation method adopted in the present application is simple to operate and has high production efficiency. The present application first premixes the polycarboxylic acid high-performance water reducer, stannous chloride, ethylene glycol butyl ether acetate and magnesium stearate intercalated hydrotalcite to ensure that these additives are evenly dispersed and give full play to their respective properties, thereby improving the impermeability, compressive strength and working performance of the concrete.

[0025] In summary, the present invention includes at least one of the following beneficial technical effects: 1. This application adopts specific raw materials and proportions to produce impermeable recycled concrete with good impermeability and high compressive strength.

[0026] 2. The present application adds magnesium stearate intercalated hydrotalcite, whose layered structure can block the penetration of water molecules, thereby improving the anti-permeability performance of concrete and also improving the compressive strength of concrete.

[0027] 3. The preparation method adopted in this application is simple to operate and has high production efficiency. DETAILED DESCRIPTION

[0028] The present application is further described in detail below with reference to the embodiments.

[0029] The present application designs an impermeable recycled concrete, which comprises, by weight, 180 to 220 parts of cement, 400 to 600 parts of recycled coarse aggregate, 200 to 300 parts of recycled fine aggregate, 100 to 150 parts of mineral admixture, 1 to 3 parts of polycarboxylic acid high-performance water reducing agent, 0.01 to 0.5 parts of stannous chloride, 0.5 to 2 parts of ethylene glycol butyl ether acetate, 1 to 5 parts of magnesium stearate intercalated hydrotalcite, and 150 to 170 parts of water.

[0030] The anti-seepage recycled concrete of the present application is prepared by the following method, comprising the following steps: S1, mixing the polycarboxylic acid high-performance water-reducing agent, stannous chloride, ethylene glycol butyl ether acetate and magnesium stearate intercalated hydrotalcite, stirring to prepare a premix; S2, mixing the recycled coarse aggregate, recycled fine aggregate and mineral admixture, stirring, adding the premix, stirring, and obtaining a mixture; S3, adding cement and water to the mixture, stirring, injecting into a mold for molding, curing, and demoulding to obtain impermeable recycled concrete.

[0031] The applicant has designed the technical solution of the present application to solve the problem that the existing concrete has insufficient impermeability and compressive strength. The obtained impermeable recycled concrete has good impermeability and high compressive strength.

[0032] The raw materials used in this application are as follows: Fly ash: Wuhan Lianhekang Biotechnology Co., Ltd., product number: A01085.

[0033] Polycarboxylic acid high performance water reducer: Huainan Kedi Chemical Technology Co., Ltd., item number: ZM-4.

[0034] Stannous chloride: CAS: 7772-99-8.

[0035] Ethylene glycol butyl ether acetate: CAS: 112-07-2.

[0036] Mg(NO3)2·6H2O (magnesium nitrate hexahydrate): CAS: 13446-18-9.

[0037] Al(NO3)3·9H2O (aluminum nitrate nonahydrate): CAS: 7784-27-2.

[0038] Magnesium stearate: CAS: 557-04-0. Specific embodiments

[0039] The preparation method of the magnesium stearate intercalated hydrotalcite used in Examples 1 to 5 is: Step 1: Mix Mg(NO3)2·6H2O and Al(NO3)3·9H2O, add water to dissolve, and prepare a mixed salt solution; Mg2+ and Al 3+ The molar ratio is 3:1; Step 2: adding a sodium hydroxide solution with a mass fraction of 5% dropwise into the mixed salt solution, stirring to generate a precipitate, filtering, washing, and drying to obtain a basic hydrotalcite; Step 3: dissolving magnesium stearate in water to prepare a magnesium stearate solution; Step 4: adding the basic hydrotalcite to the magnesium stearate solution, stirring at 80° C. for 12 hours, filtering, washing, and drying to obtain the magnesium stearate intercalated hydrotalcite; wherein the weight of the magnesium stearate accounts for 5% of the basic hydrotalcite.

[0040] Embodiments 1 to 5 The specific raw material weights of the impermeable recycled concrete prepared in Examples 1 to 5 are shown in Table 1.

[0041] Table 1 / kg Example 1 Example 2 Example 3 Example 4 Example 5 cement 220 190 200 210 180 Recycled coarse aggregate 600 550 500 450 400 Recycled fine aggregate 200 220 250 280 300 Mineral admixtures 100 110 125 140 150 Polycarboxylic acid high performance water reducing agent 1 2.5 2 1.5 3 Stannous chloride 0.1 0.2 0.3 0.4 0.5 Ethylene glycol butyl ether acetate 0.5 1.5 1.3 1 2 Magnesium stearate intercalated hydrotalcite 1 2 3 4 5 water 150 155 160 165 170 Among them, cement is P·O52.5R grade ordinary Portland cement; The recycled coarse aggregate is composed of 5-10mm and 16-25mm secondary particle sizes, with a mixing ratio of 1:2.2; the average particle size of the recycled fine aggregate is 2.7mm; The mineral admixtures are ultra-fine slag powder and fly ash in a weight ratio of 2.5:1; the specific surface area of ​​the ultra-fine slag powder is 700m 2 / kg, and the loss on ignition is 1.6%.

[0042] The preparation method of Example 1 comprises the following steps: S1. Mixing a polycarboxylic acid high-performance water-reducing agent, stannous chloride, ethylene glycol butyl ether acetate and magnesium stearate intercalated hydrotalcite, stirring to prepare a premix; S2. Mix the recycled coarse aggregate, recycled fine aggregate and mineral admixture, stir, add premix, stir to obtain a mixture; S3. Add cement and water to the mixture, stir, inject into a mold for molding, cure, and demould to obtain impermeable recycled concrete.

[0043] The preparation methods of Examples 2 to 5 are consistent with that of Example 1.

[0044] Comparative Examples 1 to 6 Comparative Example 1 The difference between Comparative Example 1 and Example 3 is that in Comparative Example 1, no stannous chloride, ethylene glycol butyl ether acetate and magnesium stearate intercalated hydrotalcite are added.

[0045] Comparative Example 2 The difference between Comparative Example 2 and Example 3 is that in Comparative Example 2, no stannous chloride and magnesium stearate intercalated hydrotalcite are added.

[0046] Comparative Example 3 The difference between Comparative Example 3 and Example 3 is that no stannous chloride is added in Comparative Example 3.

[0047] Comparative Example 4 The difference between Comparative Example 4 and Example 3 is that, in Comparative Example 4, magnesium stearate intercalated hydrotalcite is not added.

[0048] Comparative Example 5 The difference between Comparative Example 5 and Example 3 is that the preparation method of Comparative Example 5 is: S1. Mixing recycled coarse aggregate, recycled fine aggregate, mineral admixture, polycarboxylic acid high-performance water reducing agent, stannous chloride, ethylene glycol butyl ether acetate and magnesium stearate intercalated hydrotalcite, stirring to prepare a mixture; S2. Add cement and water to the mixture, stir, inject into a mold for molding, cure, and demould to obtain impermeable recycled concrete.

[0049] Comparative Example 6 The difference between Comparative Example 6 and Example 3 is that in Comparative Example 6, the magnesium stearate intercalated hydrotalcite is replaced with an equal weight of basic hydrotalcite, and the preparation method of the basic hydrotalcite is: Step 1: Mix Mg(NO3)2·6H2O and Al(NO3)3·9H2O, add water to dissolve, and prepare a mixed salt solution; Mg 2+ and Al 3+ The molar ratio is 3:1; Step 2: adding a sodium hydroxide solution with a mass fraction of 5% dropwise into the mixed salt solution, stirring, generating a precipitate, filtering, washing, and drying to obtain a basic hydrotalcite.

[0050] Experimental testing Test items and test methods: Water seepage performance: The water seepage height of water-resistant recycled concrete is measured according to the water seepage height method 6.1 in GB / T 50082-2009 "Standard for test methods of long-term performance and durability of ordinary concrete"; Compressive strength: The compressive strength of impermeable recycled concrete is determined according to GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete".

[0051] The impermeability and compressive strength of the impermeable recycled concrete prepared in Examples 1 to 5 and Comparative Examples 1 to 6 were tested. The test results are shown in Table 2.

[0052] Table 2 From the test results in Table 2, it can be seen that the impermeable recycled concretes prepared in Examples 1 to 5 have good impermeability and high compressive strength, among which the impermeability and compressive strength of the impermeable recycled concrete prepared in Example 3 are the highest.

[0053] In Comparative Example 1, stannous chloride, ethylene glycol butyl ether acetate and magnesium stearate intercalated hydrotalcite were not added, and the impermeability and compressive strength of the obtained impermeable recycled concrete were significantly reduced.

[0054] The impermeability and compressive strength of the impermeable concrete prepared in Comparative Examples 2 to 4 are inferior to those in Example 3.

[0055] In Comparative Example 5, the polycarboxylic acid high-performance water-reducing agent, stannous chloride, ethylene glycol butyl ether acetate and magnesium stearate intercalated hydrotalcite were not premixed, and the impermeability and compressive strength of the obtained impermeable concrete were not as good as those in Example 3.

[0056] In Comparative Example 6, the magnesium stearate intercalated hydrotalcite was replaced with an equal weight of basic hydrotalcite, and the impermeability and compressive strength of the obtained impermeable concrete were lower than those of Example 3.

[0057] Embodiments 6 to 13 Example 6 The difference between Example 6 and Example 3 is that in Example 6, the recycled coarse aggregate is composed of secondary particle sizes of 5-10 mm and 16-25 mm, and the blending ratio is 1:1.5.

[0058] Example 7 The difference between Example 7 and Example 3 is that in Example 7, the recycled coarse aggregate is composed of secondary particle sizes of 5-10 mm and 16-25 mm, and the blending ratio is 1:3.

[0059] Example 8 The difference between Example 8 and Example 3 is that in Example 8, the average particle size of the recycled fine aggregate is 2 mm.

[0060] Example 9 The difference between Example 9 and Example 3 is that in Example 9, the average particle size of the recycled fine aggregate is 3.5 mm.

[0061] Example 10 The difference between Example 10 and Example 3 is that in Example 10, the weight ratio of ultrafine slag powder to fly ash is 2:1.

[0062] Embodiment 11 The difference between Example 11 and Example 3 is that in Example 11, the weight ratio of ultrafine slag powder to fly ash is 3:1.

[0063] Example 12 The difference between Example 12 and Example 3 is that in Example 12, the weight ratio of stannous chloride and magnesium stearate intercalated hydrotalcite is 1:8, and the total weight of stannous chloride and magnesium stearate intercalated hydrotalcite is 3.3 kg.

[0064] Embodiment 13 The difference between Example 13 and Example 3 is that in Example 13, the weight ratio of stannous chloride and magnesium stearate intercalated hydrotalcite is 1:12, and the total weight of stannous chloride and magnesium stearate intercalated hydrotalcite is 3.3 kg.

[0065] The impermeability and compressive strength of the impermeable recycled concrete prepared in Examples 6 to 13 were tested. The test results are shown in Table 3.

[0066] Table 3 28d water seepage height / mm 7d compressive strength / MPa 28d compressive strength / MPa Example 6 50 36.0 50.9 Example 7 54 35.4 49.7 Example 8 48 36.3 51.3 Example 9 53 35.7 49.9 Example 10 55 35.1 49.5 Embodiment 11 51 35.6 50.2 Example 12 48 36.1 51.0 Embodiment 13 50 35.7 49.5 From the test results in Table 3, it can be seen that the difference between Example 6 and Example 7 and Example 3 is that the mixing ratio of the recycled coarse aggregate is different, among which the impermeability and compressive strength of the impermeable recycled concrete prepared in Example 3 are the best.

[0067] The difference between Example 8 and Example 9 and Example 3 is that the average particle size of the recycled fine aggregate is different. Among them, the impermeability and compressive strength of the impermeable recycled concrete prepared in Example 3 are the best.

[0068] The difference between Example 10 and Example 11 and Example 3 is that the weight ratios of ultrafine slag powder and fly ash are different. Among them, the impermeability and compressive strength of the impermeable recycled concrete prepared in Example 3 are the best.

[0069] The difference between Example 12 and Example 13 and Example 3 is that the weight ratios of stannous chloride and magnesium stearate intercalated hydrotalcite are different. Among them, the impermeability and compressive strength of the impermeable recycled concrete prepared in Example 3 are the best.

[0070] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. An anti-seepage recycled concrete, It is characterized in that Calculated by weight, the raw material composition includes: 180-220 parts of cement, 400-600 parts of recycled coarse aggregate, 200-300 parts of recycled fine aggregate, 100-150 parts of mineral admixture, 1-3 parts of polycarboxylic acid high-performance water reducer, 0.1-0.5 parts of stannous chloride, 0.5-2 parts of ethylene glycol butyl ether acetate, 1-5 parts of magnesium stearate intercalated hydrotalcite, and 150-170 parts of water.

2. The anti-seepage recycled concrete according to claim 1, It is characterized in that The raw material composition includes, by weight: 190-210 parts of cement, 450-550 parts of recycled coarse aggregate, 220-280 parts of recycled fine aggregate, 110-140 parts of mineral admixture, 1.5-2.5 parts of polycarboxylic acid high-performance water reducer, 0.2-0.4 parts of stannous chloride, 1-1.5 parts of ethylene glycol butyl ether acetate, 2-4 parts of magnesium stearate intercalated hydrotalcite, and 155-165 parts of water.

3. The anti-seepage recycled concrete according to claim 1, It is characterized in that The raw material composition includes, by weight: 200 parts of cement, 500 parts of recycled coarse aggregate, 250 parts of recycled fine aggregate, 125 parts of mineral admixture, 2 parts of polycarboxylic acid high-performance water reducer, 0.3 parts of stannous chloride, 1.3 parts of ethylene glycol butyl ether acetate, 3 parts of magnesium stearate intercalated hydrotalcite, and 160 parts of water.

4. The anti-seepage recycled concrete according to claim 1, It is characterized in that The recycled coarse aggregate is composed of two-level particle sizes of 5-10 mm and 16-25 mm, and the blending ratio is 1:1.5-3.

5. The anti-seepage recycled concrete according to claim 1, It is characterized in that The average particle size of the recycled fine aggregate is 2-3.5 mm.

6. The anti-seepage recycled concrete according to claim 1, It is characterized in that The mineral admixture comprises ultrafine slag powder and fly ash, and the weight ratio of the ultrafine slag powder to the fly ash is 2-3:

1.

7. The anti-seepage recycled concrete according to claim 1, It is characterized in that The specific surface area of ​​the ultrafine slag powder is not less than 700m 2 / kg, loss on ignition is not more than 1.6%.

8. The anti-seepage recycled concrete according to claim 1, It is characterized in that The preparation method of the magnesium stearate intercalated hydrotalcite is: Step 1: Mg(NO 3 ) 2 6H 2 O and Al (NO 3 ) 3 9H 2 O mixed, added water to dissolve, to prepare a mixed salt solution; Mg 2+ and Al 3+ The molar ratio is 2~3:1; Step 2: adding a sodium hydroxide solution dropwise to the mixed salt solution, stirring to generate a precipitate, filtering, washing, and drying to obtain a basic hydrotalcite; Step 3: dissolving magnesium stearate in water to prepare a magnesium stearate solution; Step 4: adding the basic hydrotalcite to the magnesium stearate solution, stirring at 80-90° C. for 4-20 hours, filtering, washing, and drying to obtain the magnesium stearate intercalated hydrotalcite.

9. The anti-seepage recycled concrete according to claim 1, It is characterized in that The weight ratio of the stannous chloride to the magnesium stearate intercalated hydrotalcite is 1:8-12.

10. A method for preparing the impermeable recycled concrete according to claim 1, It is characterized in that The following steps are involved: S1, mixing the polycarboxylic acid high-performance water-reducing agent, stannous chloride, ethylene glycol butyl ether acetate and magnesium stearate intercalated hydrotalcite, stirring to prepare a premix; S2, mixing the recycled coarse aggregate, recycled fine aggregate and mineral admixture, stirring, adding the premix, stirring, and obtaining a mixture; S3, adding cement and water to the mixture, stirring, injecting into a mold for molding, curing, and demoulding to obtain impermeable recycled concrete.