Method for improving warping of DCB low-thickness product during sintering
By bonding porcelain strips on the surface of the pad and supporting columns on the center point, the warping problem during sintering of DCB products is solved, and the heat distribution is achieved, the warping and processing cost are reduced, and the product is improved. Pass rate.
Patent Information
- Application Number
- CN202411233495.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-12-03
AI Technical Summary
During the sintering process, DCB products are not easy to control due to the difference in thermal expansion coefficients of copper sheets and porcelain sheets, which are prone to product distortion and porcelain cracks, which are too large, affecting the subsequent welding quality.
The first and second porcelain strips are bonded around the surface of the pad, and the support columns are bonded at the center of the pad to form a sintering fixture. The porcelain pieces and copper foil are placed in the fixture in turn to cover copper. Sintering ensures uniform distribution of heat and reduces warpage.
Through uniform thermal distribution and support, the warpage of DCB products is reduced, the product pass rate is improved, and the processing cost is reduced.
Smart Images

Figure CN119059835A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor manufacturing technology, and in particular to a method for improving the warping of a low-thickness DCB product during sintering. Background Art
[0002] DCB technology uses copper's oxygen-containing eutectic liquid to directly bond copper to ceramics. The basic principle is to introduce an appropriate amount of oxygen between copper and ceramic (alumina) before or during the bonding process. Within a certain temperature range, copper and oxygen form a Cu-O eutectic liquid, which infiltrates the copper foil to achieve the bonding of the ceramic substrate and the copper plate to generate copper aluminate and copper aluminate.
[0003] During the sintering process of copper-clad ceramic substrates, due to the large difference in thermal expansion coefficients between the copper sheet and the ceramic sheet, the ceramic sheet is subjected to a large tensile force from the copper surfaces on both sides during the sintering process. The warping value is difficult to control, and product distortion and ceramic cracking are prone to occur. The sintered DCB product has excessive warping, which causes voids in the subsequent welding of the product. Summary of the invention
[0004] The object of the present invention is to provide a method for improving the warping of low-thickness DCB products during sintering, by first bonding a pad, a first porcelain strip, and a second porcelain strip, and then bonding a support column at the center point of the pad to form a sintering jig, placing porcelain sheets and copper sheets in the sintering jig in sequence, and performing sintering of the first copper-clad surface and the second copper-clad surface, thereby reducing the warping of the DCB product obtained by sintering, and solving the above-mentioned problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention adopts the following solutions: A method for improving the warpage of a low-thickness DCB product during sintering, comprising the following steps: Step 1: bonding the first ceramic strip and the second ceramic strip around the surface of the backing plate, and then bonding the support column at the center point of the backing plate to form a sintering fixture; Step 2, placing the ceramic sheet to be sintered and the copper foil in the sintering fixture in sequence, and after the placement is completed, performing first-side copper-clad sintering to obtain a single-side copper-clad semi-finished product; The thickness of the ceramic sheet is less than 0.32 mm; Step three, turning over the single-sided copper-clad semi-finished product in step two and placing it in the sintering jig, placing copper foil on top of the single-sided copper-clad semi-finished product, and then performing second-sided copper-clad sintering.
[0006] The technical concept of the present application is: by bonding the first porcelain strip and the second porcelain strip around the surface of the pad, the second porcelain strip is located between the ends of the two first porcelain strips, and bonding the support column at the center point of the pad to form a sintering jig, and under the combination of the first porcelain strip and the second porcelain strip of a specific thickness, the porcelain sheet and the copper foil are placed in the sintering jig, and the first-side copper-clad sintering and the second-side copper-clad sintering are performed, so that the DCB product is evenly heated and stressed during the sintering process, the deformation during the heating process is more uniform, and it is not easy to produce distortion at high temperatures to cause porcelain cracks, thereby reducing the warping of the product.
[0007] Further preferably, before performing step 2, the sintering jig is placed above the conveyor belt of the tunnel furnace, and the bottom surface of the pad is in contact with the surface of the conveyor belt, so as to prevent the ceramic sheet from contacting the conveyor belt of the tunnel furnace and causing contamination, and at the same time, the pad prevents the heat generated in the tunnel furnace from being quickly transferred to the ceramic sheet, thereby preventing the DCB product from being deformed due to excessive heating.
[0008] Further preferably, the pad is a rectangular parallelepiped, the first ceramic strip is bonded to the long side of the pad surface, the second ceramic strip is bonded to the short side of the pad surface, the two ends of the second ceramic strip are located between the ends of the two first ceramic strips, and the raw materials of the pad, the first ceramic strip, the second ceramic strip and the support column all include 96% by mass of Al 2 O 3 Ceramics, 1.5%~2.3% SiO by mass 2 , the balance is magnesium and calcium.
[0009] Further preferably, the bonding uses high temperature resistant infinite glue.
[0010] Further preferably, the bottom surfaces of the ceramic sheet and the single-sided copper-clad semi-finished product are in contact with the support pillars respectively.
[0011] Further preferably, the pad has a length of 190 mm, a width of 138 mm, and a thickness of 1 mm.
[0012] Further preferably, the first ceramic strip has a length of 190 mm, a width of 3 mm, and a thickness of 2 mm to 4 mm.
[0013] The second ceramic strip has a length of 132 mm, a width of 3 mm, and a thickness of 2 mm to 4 mm; Further preferably, the support column has a length of 3 mm, a width of 3 mm, and a thickness of 2 mm.
[0014] Further preferably, the sintering temperature of the first-side copper cladding and the second-side copper cladding is 1065° C. to 1078° C., and the belt speed of the conveyor belt is 100 mm / min to 160 mm / min.
[0015] Further preferably, during the sintering process of the first-side copper coating and the second-side copper coating, the sintering jig passes through four temperature rising zones, four constant temperature zones and three temperature falling zones in sequence; The four temperature rising zones are set at 600℃~700℃, 700℃~850℃, 850℃~960℃, and 850℃~1050℃ respectively; The total length of the heating zone is 1000~1200mm; the time for the sintering fixture to pass through the heating zone is 9~15min; The passing time of the four heating zones is 3~4.5min, 3~4.5min, 3~4.5min, 3~4.5min, respectively; The temperature of the four constant temperature zones is set between 1070℃ and 1075℃; the total length of the constant temperature zones is 1300~1500mm; the time for the sintering fixture to pass through the constant temperature zones is 14~18min; The three cooling zones are set at temperatures between 1025℃~1035℃, 970℃~980℃, and 920℃~930℃ respectively; The total length of the cooling zone is 1000~1100mm; the time for the sintering fixture to pass through the cooling zone is 9~13min.
[0016] The beneficial effects of the present invention are as follows: the present invention is a method for improving the warping of low-thickness DCB products during sintering, by arranging the first ceramic strip and the second ceramic strip around the surface of the pad, and combining them with the support column arranged at the center point of the pad, so that the product is evenly stressed on the jig, the pad reduces the heat transfer from the tunnel furnace to the product, making the product more uniform during the deformation process, and not prone to distortion at high temperatures to cause ceramic cracks, reducing the warping of the product, improving the product qualification rate, and reducing the processing cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is a schematic diagram of the structure of a sintering fixture according to Example 1 of the present invention; Figure 2 This is a top view of the sintering fixture according to Example 1 of the present invention.
[0018] Figure numerals: 1- pad, 2- first ceramic strip, 3- second ceramic strip, 4- support column, 5- transmission belt, 6- ceramic sheet, 7- copper foil. DETAILED DESCRIPTION
[0019] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described below in conjunction with the drawings of the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] Example 1 A method for improving the warpage of a low-thickness DCB product during sintering, comprising the following steps: Step 1: Bond the first ceramic strip and the second ceramic strip around the surface of the pad, and then bond the support column at the center point of the pad to form a sintering fixture; refer to Figure 1 and Figure 2 .
[0021] The pad is a rectangular parallelepiped, the first ceramic strip is bonded to the long side of the pad surface, the second ceramic strip is bonded to the short side of the pad surface, and the two ends of the second ceramic strip are located between the ends of the two first ceramic strips.
[0022] Further preferably, the bonding uses high temperature resistant infinite glue.
[0023] Further preferably, the bottom surfaces of the ceramic sheet and the single-sided copper-clad semi-finished product are in contact with the support pillars respectively.
[0024] Further preferably, the pad has a length of 190 mm, a width of 138 mm, and a thickness of 1 mm.
[0025] Further preferably, the first ceramic strip has a length of 190 mm, a width of 3 mm, and a thickness of 2 mm to 4 mm.
[0026] The second ceramic strip has a length of 132 mm, a width of 3 mm, and a thickness of 2 mm to 4 mm.
[0027] The support column has a length of 3 mm, a width of 3 mm, and a thickness of 2 mm. The raw materials of the backing plate, the first ceramic strip, the second ceramic strip and the support column all include 96% by mass of Al 2 O 3 Ceramics, 1.5%~2.3% SiO by mass 2 , the balance is magnesium and calcium.
[0028] Further preferably, before performing step 2, the sintering jig is placed above the conveyor belt of the tunnel furnace, and the bottom surface of the pad is in contact with the surface of the conveyor belt, so as to prevent the ceramic sheet from contacting the conveyor belt of the tunnel furnace and causing contamination, and at the same time, the pad prevents the heat generated in the tunnel furnace from being quickly transferred to the ceramic sheet, thereby preventing the DCB product from being deformed due to excessive heating.
[0029] Step 2, placing the ceramic sheet to be sintered and the copper foil in the sintering fixture in sequence, and after the placement is completed, performing first-side copper-clad sintering to obtain a single-side copper-clad semi-finished product; The thickness of the ceramic sheet is less than 0.32 mm; Step three, turning over the single-sided copper-clad semi-finished product in step two and placing it in the sintering jig, placing copper foil on top of the single-sided copper-clad semi-finished product, and then performing second-sided copper-clad sintering.
[0030] The sintering temperature of the first copper-clad surface and the second copper-clad surface is 1065° C. to 1078° C., and the belt speed of the conveyor belt is 100 mm / min to 160 mm / min.
[0031] During the sintering process of the first copper-clad surface and the second copper-clad surface, the sintering fixture passes through four temperature-increasing zones, four constant temperature zones and three temperature-decreasing zones in sequence; The four temperature rising zones are set at 600℃~700℃, 700℃~850℃, 850℃~960℃, and 850℃~1050℃ respectively; The total length of the heating zone is 1000~1200mm; the time for the sintering fixture to pass through the heating zone is 9~15min; The passing time of the four heating zones is 3~4.5min, 3~4.5min, 3~4.5min, 3~4.5min, respectively; The temperature of the four constant temperature zones is set between 1070℃ and 1075℃; the total length of the constant temperature zones is 1300~1500mm; the time for the sintering fixture to pass through the constant temperature zones is 14~18min; The three cooling zones are set at temperatures between 1025℃~1035℃, 970℃~980℃, and 920℃~930℃ respectively; The total length of the cooling zone is 1000~1100mm; the time for the sintering fixture to pass through the cooling zone is 9~13min.
[0032] Comparative Example 1 Comparative Example 1 of the present application adopts the sintering process of Example 1, placing the ceramic sheet and the copper foil into the sintering fixture in sequence, and performing first-side copper-clad sintering and second-side copper-clad sintering respectively.
[0033] The main difference is that the thickness of the first porcelain strip and the second porcelain strip of the sintering fixture are both less than 2 mm.
[0034] Comparative Example 2 Comparative Example 2 of the present application adopts the sintering process of Example 1, placing the ceramic sheet and the copper foil into the sintering fixture in sequence, and performing first-side copper-clad sintering and second-side copper-clad sintering respectively.
[0035] The main difference is that the thickness of the first porcelain strip and the second porcelain strip of the sintering fixture are both greater than 4 mm.
[0036] Table 1 Comparison of product yield and warpage after sintering of Example 1 of the present invention and Comparative Example 1 and Comparative Example 2 According to Table 1, the product yield and warpage of the final product obtained by sintering with the sintering jig of the present invention in Example 1 are significantly better than those in Comparative Examples 1 and 2, which means that the first and second porcelain strips are arranged around the surface of the pad, and are combined with the support column arranged at the center of the pad. At the same time, the thickness of the first and second porcelain strips is between 2 mm and 4 mm, so that the product is evenly stressed on the jig. The pad reduces the heat transfer in the tunnel furnace to the product, making the product more uniform during the deformation process, and is not prone to distortion at high temperatures, thereby causing porcelain cracks, thereby improving the product qualification rate and reducing processing costs.
[0037] The above description is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present invention. Although the present invention has been disclosed as a preferred embodiment as above, it is not intended to limit the present invention. Any technician familiar with the profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.
Claims
1. A method for improving the warpage of low-thickness DCB products during sintering, characterized in that: The following steps are involved: Step 1: bonding the first ceramic strip and the second ceramic strip around the surface of the backing plate, and then bonding the support column at the center point of the backing plate to form a sintering fixture; Step 2, placing the ceramic sheet to be sintered and the copper foil in the sintering fixture in sequence, and after the placement is completed, performing first-side copper-clad sintering to obtain a single-side copper-clad semi-finished product; The thickness of the ceramic sheet is less than 0.32 mm; Step three, turning over the single-sided copper-clad semi-finished product in step two and placing it in the sintering jig, placing copper foil on top of the single-sided copper-clad semi-finished product, and then performing second-sided copper-clad sintering.
2. A method for improving the warpage of low-thickness DCB products during sintering according to claim 1, characterized in that: Before performing step 2, the sintering jig is placed above the conveyor belt of the tunnel furnace, and the bottom surface of the pad is in contact with the surface of the conveyor belt.
3. The method for improving the warpage of low-thickness DCB products during sintering according to claim 1, characterized in that: The pad is a rectangular parallelepiped, the first ceramic strip is bonded to the long side of the pad surface, the second ceramic strip is bonded to the short side of the pad surface, and the two ends of the second ceramic strip are located between the ends of the two first ceramic strips. The raw materials of the pad, the first ceramic strip, the second ceramic strip and the support column all include 96% Al2O3 ceramic by mass, 1.5%~2.3% SiO2 by mass, and the remainder is magnesium and calcium.
4. The method for improving the warpage of low-thickness DCB products during sintering according to claim 1, characterized in that: The bonding adopts high temperature resistant infinite glue.
5. The method for improving the warpage of low-thickness DCB products during sintering according to claim 1, characterized in that: The bottom surfaces of the ceramic sheet and the single-sided copper-clad semi-finished product are in contact with the supporting pillars respectively.
6. The method for improving the warpage of low-thickness DCB products during sintering according to claim 1, characterized in that: The pad has a length of 190 mm, a width of 138 mm and a thickness of 1 mm.
7. The method for improving the warpage of low-thickness DCB products during sintering according to claim 1, characterized in that: The first ceramic strip has a length of 190 mm, a width of 3 mm, and a thickness of 2 mm to 4 mm; The second ceramic strip has a length of 132 mm, a width of 3 mm, and a thickness of 2 mm to 4 mm.
8. The method for improving the warpage of low-thickness DCB products during sintering according to claim 1, characterized in that: The support column has a length of 3 mm, a width of 3 mm, and a thickness of 2 mm.
9. The method for improving the warpage of low-thickness DCB products during sintering according to claim 1, characterized in that: The sintering temperature of the first copper-clad surface and the second copper-clad surface is 1065° C. to 1078° C., and the belt speed of the conveyor belt is 100 mm / min to 160 mm / min.
10. The method for improving the warpage of low-thickness DCB products during sintering according to claim 1, characterized in that: During the sintering process of the first copper-clad surface and the second copper-clad surface, the sintering fixture passes through four temperature-increasing zones, four constant temperature zones and three temperature-decreasing zones in sequence; The four temperature rising zones are set at 600℃~700℃, 700℃~850℃, 850℃~960℃, and 850℃~1050℃ respectively; The total length of the heating zone is 1000~1200mm; the time for the sintering fixture to pass through the heating zone is 9~15min; The passing time of the four heating zones is 3~4.5min, 3~4.5min, 3~4.5min, 3~4.5min, respectively; The temperature of the four constant temperature zones is set between 1070℃ and 1075℃; the total length of the constant temperature zones is 1300~1500mm; the time for the sintering fixture to pass through the constant temperature zones is 14~18min; The three cooling zones are set at temperatures between 1025℃~1035℃, 970℃~980℃, and 920℃~930℃ respectively; The total length of the cooling zone is 1000~1100mm; the time for the sintering fixture to pass through the cooling zone is 9~13min.
Citation Information
Patent Citations
Method for improving poor warping of DCB substrate during sintering
CN115938953A
Double-sided sintering jig for controlling warping amount of DBC (Direct Bonding Copper)
CN214142120U
Single-sided sintering jig for copper-clad ceramic substrate
CN216144176U
Sintering jig for copper-clad ceramic substrate
CN219511279U
Ceramic circuit board and semiconductor module
JP2006237383A