Diamine mono-boron compound, derivative polymer thereof and application of diamine mono-boron compound and derivative polymer thereof in OLED (Organic Light Emitting Diode) field
By designing diamine monoborate compounds and their derived polymers with specific chemical structures, the problems of low color purity and poor dielectric properties of OLED materials are solved, and high-efficiency blue-violet light narrow emission and excellent dielectric properties of OLED are achieved. Device.
Patent Information
- Application Number
- CN202411183910.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-27
AI Technical Summary
Existing OLED materials face the problem of excessively wide half-maximum width of the emission spectrum, resulting in poor dielectric performance of MR-TADF molecules and flexible OLED substrates that lack high-performance blue-violet emission.
By designing diamine monoborate compounds with specific chemical structures and their derived polymers, using the B-N resonance effect and the interaction between long-range charge transfer states and short-range charge transfer states, the orbital spin coupling constant between ground states and excited states is achieved, and Narrow-emitting blue-violet OLED devices, and improve the dielectric and optical properties of OLED devices through strong electron donor peripheral modification and large-volume side-based structure.
The blue-violet narrow-emitting OLED device with high efficiency and low driving voltage is realized, which improves color purity and dielectric performance, and improves the optical transparency and dielectric performance of the flexible OLED substrate.
Smart Images

Figure CN119060078A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of organic photoelectric materials and their applications, and more specifically, relates to a class of diamine monoboron compounds and their derivative polymers and their applications in the field of OLED. Background Art
[0002] Organic electroluminescent technology (OLED) has been widely used in the display field due to its outstanding advantages such as self-luminescence, fast response speed, and flexible foldability. At the same time, with the continuous development of OLED-related technologies and the continuous improvement of consumers' requirements for product performance, organic light-emitting materials currently generally face the problem of too wide half-maximum width (FWHM) of the emission spectrum (70-100nm), so OLED cannot directly achieve high color purity display, and corresponding solutions are urgently needed.
[0003] The third generation of thermally activated delayed fluorescence materials (TADF) achieves 100% internal quantum efficiency in organic small molecules, and is expected to replace existing traditional fluorescent materials and phosphorescent materials, with advantages in cost and efficiency. However, TADF materials generally have strong structural relaxation characteristics due to their molecular design, which causes their luminescence spectrum half-width (FWHM) to be usually above 70nm, greatly affecting the color purity of OLED devices. To solve this problem, Professor T. Hatakeyama of Kwansei Gakuin University and others developed a thermally activated delayed fluorescence material (MR-TADF) with multiple induced resonance characteristics. The principle is to achieve the separation of molecular HOMO / LUMO at the atomic scale through the opposite resonance effects of electron-deficient atoms (B) and electron-rich atoms (N), thereby obtaining an extremely narrow FWHM while maintaining the characteristics of TADF materials. However, most of the MR-TADF molecules reported so far use weak donors or acceptors to modify the resonance skeleton, which makes the frontier orbital energy level distribution dominated by short-range charge transfer states (SRCT), resulting in weak orbital spin coupling (SOC) between the ground state and the excited state, which limits the performance of OLED devices based on MR-TADF molecules. At the same time, weak donors or acceptors make it difficult to significantly adjust the light color of MR-TADF molecules. Most MR-TADF molecules emit sky blue or green light, which makes it very difficult to have high-performance, blue-violet light-emitting MR-TADF molecules at this stage.
[0004] The research group of the inventor of the present invention has obtained a class of monoboron derivatives based on fluorene-aniline fusion donors, their preparation and application (see Chinese patent CN 202210431760.2 for details). It introduces rigid group fluorene derivatives on the basis of retaining electron-rich N atoms to form new fusion donors. This type of fusion donor based on fluorene-aniline has the characteristics of rigidity and large volume, and obtains monoboron derivatives based on fluorene-aniline fusion donors. Based on the BN resonance effect, FWHM below 30nm can be achieved, which can effectively improve the color purity of OLED devices. However, the emission wavelength of this series of monoboron derivatives is 440nm to 500nm, and the light color is still difficult to meet the BT.2020 blue light standard issued by the International Telecommunication Union Radiocommunication Sector (ITU-R). In fact, the currently reported narrow-emission boron-nitrogen derivatives are almost unable to possess the blue-violet light color (in this field, the wavelength of "blue-violet light" is 400nm to 430nm) (ref: Chinese Journal of Organic Chemistry 2023, 43(5)1645-1690), so it is urgent to explore high-performance, blue-violet light-emitting MR-TADF molecules.
[0005] In addition, in recent years, polyimide films are often used as the preferred material for OLED flexible substrates because polyimide has excellent thermal stability, chemical stability, mechanical properties, etc. However, the dielectric constant and dielectric loss of traditional polyimide are generally high. Taking commercial Kapton film as an example, at 10GHz, its dielectric constant (D k ) value is 3.4, dielectric loss (D f ) value is 0.016, which can easily lead to serious transmission loss in OLED devices. In addition, charge transfer complexes are easily formed between polyimide molecular chains, which often makes the optical transparency of the film poor, which can easily affect the overall performance of OLED devices. Therefore, how to improve the dielectric and optical properties of polyimide film substrates has become a hot topic in research. Summary of the invention
[0006] In view of the above defects or improvement needs of the prior art, the purpose of the present invention is to provide a class of diamine monoboron compounds and their derivative polymers and their applications in the field of OLED, wherein the chemical structure of the diamine monoboron compound is improved to form general formulas A-1 to A-4 with specific chemical structures (the R1 and R2 groups in each general formula meet the requirements of the specific group), and the corresponding diamine monoboron compound can be applied to the light-emitting layer of the OLED device, and the derived polyimide polymer can be applied to the OLED flexible substrate. Based on the BN resonance effect and the interaction between the long-range charge transfer state and the short-range charge transfer state, the orbital spin coupling constant between the ground state and the excited state is improved, and the diamine monoboron compound can effectively improve the color purity of the OLED device, and prepare a blue-violet light (i.e., 400nm to 430nm) and narrow emission (half-maximum width FWHM is less than 30nm) OLED device with high efficiency and low driving voltage; based on the extremely rigid bulky side group structure and the improved polymer free volume, the polyimide polymer derived from the diamine monoboron compound is conducive to the preparation of a flexible OLED substrate with excellent optical and dielectric properties.
[0007] To achieve the above object, according to one aspect of the present invention, a diamine monoboron compound is provided, characterized in that the diamine monoboron compound has a general structure as shown in at least one of the general formulas A-1 to A-4,
[0008]
[0009] wherein R1 and R2 are independently selected from hydrogen, deuterium, methyl, phenyl, methoxy, trifluoromethyl, tert-butyl, naphthyl, anthracenyl, silane, halogen, pyrazine, pyridine, pyrimidine, benzimidazole ring, carbazole, indolecarbazole, phenoxazine, phenothiazine, phenoselenazine, phenanthroimidazole, substituted or unsubstituted C2-C 10 Straight chain alkyl, substituted or unsubstituted C2~C 10 Branched alkyl, substituted or unsubstituted C7~C 30 Aryl, substituted or unsubstituted C2~C 10 Alkoxy, substituted or unsubstituted C1~C 10 Alkylamino, substituted or unsubstituted C2~C 10 Silane group.
[0010] As a further preference of the present invention, the R1 group is selected from hydrogen, methyl, phenyl, trifluoromethyl, tert-butyl, halogen, pyrazine, pyridine, pyrimidine, phenoxazine, phenothiazine, phenoselenazine; the R2 group is selected from hydrogen, methyl, trifluoromethyl, tert-butyl, halogen.
[0011] As a further preferred embodiment of the present invention, the structural formula of the diamine monoboron compound is shown in any one of Formula 1 to Formula 144:
[0012]
[0013]
[0014]
[0015]
[0016]
[0017] According to another aspect of the present invention, the present invention provides a polyimide polymer derived from the above-mentioned diamine monoboron compound, characterized in that the polyimide polymer has a general structure as shown in at least one of the general formulas B-1 to B-4:
[0018]
[0019] Wherein, Ar is a tetravalent aromatic group; n is a natural number from 1 to 1000;
[0020] The general formula B-1 is constructed from a diamine monoboron compound satisfying the general formula A-1;
[0021] The general formula B-2 is constructed from a diamine monoboron compound satisfying the general formula A-2;
[0022] The general formula B-3 is constructed by a diamine monoboron compound satisfying the general formula A-3;
[0023] The general formula B-4 is constructed from a diamine monoboron compound satisfying the general formula A-4.
[0024] As further preferred of the present invention, Ar is selected from:
[0025]
[0026] According to another aspect of the present invention, the present invention provides use of the above-mentioned diamine monoboron compound and / or the above-mentioned polyimide polymer in an organic electroluminescent device.
[0027] As a further preferred embodiment of the present invention, the diamine monoboron compound is specifically used as a guest luminescent material in the light-emitting layer of an organic electroluminescent device;
[0028] The polyimide polymer is specifically used as a thin film material in a flexible substrate of an organic electroluminescent device.
[0029] As a further preferred embodiment of the present invention, the organic electroluminescent device comprises in sequence: an anode, a hole injection layer, a hole transport layer, a light emitting layer, an electron transport layer, an electron injection layer, and a cathode;
[0030] Preferably, an electron blocking layer or an exciton blocking layer is further provided between the hole transport layer and the light emitting layer; and a hole blocking layer or an exciton blocking layer is further provided between the light emitting layer and the electron transport layer.
[0031] Through the above technical scheme conceived by the present invention, compared with the reported MR-TADF compounds, the diamine monoboron compound in the present invention has multiple induced resonance effects, thermal delayed fluorescence characteristics and LRCT / SRCT interactions, which can differentiate the singlet and triplet energy levels, achieve narrowing of the half-peak width of the luminescence spectrum and efficient fluorescence emission, and be used as an organic fluorescent luminescent material in the light-emitting layer structure of an organic electroluminescent device (OLED), which is beneficial to improving the OLED luminescent color purity and significantly blue-shifting the light color, which is beneficial to the preparation of high-performance blue-violet narrow-emission OLED devices. In addition, compared with the reported flexible OLED polyimide substrate, the polyimide derived from the diamine monoboron compound in the present invention has extremely rigid large-volume side groups and increased free volume, which inhibits the formation of charge transfer complexes in the molecular chain, thereby reducing the dielectric constant and dielectric loss of the polyimide substrate and improving its optical transparency.
[0032] Moreover, compared with the previous study CN 202210431760.2, the previous study was based on the short-range charge transfer state of the boron nitrogen skeleton. The weak donor group was introduced, which made it difficult to significantly change the electron cloud of the boron nitrogen parent nucleus, and therefore it was difficult to prepare blue-violet light materials. On the basis of the short-range charge transfer state, the present invention introduces a long-range charge transfer state through a strong electron-donating amino group, which greatly weakens the electron-withdrawing energy of the boron atom, thereby greatly blue-shifting the light color. In addition, due to the interaction between the long-range charge transfer state and the short-range charge transfer state, the spin coupling between the triplet state and the singlet state is enhanced, so the luminescence efficiency of the material is also improved.
[0033] The present invention uses a multi-resonance mother core based on a boron-nitrogen structure, which can achieve a FWHM below 30nm and effectively improve the color purity of OLED devices. The strong electron donor is modified peripherally to form a strong N-π-B structure, which effectively weakens the electron-withdrawing ability of the B atom, thereby causing a significant blue shift in the light color. At the same time, the introduction of a strong power-supplying amino group enhances the long-range charge transfer state (LRCT), forms an LRCT / SRCT interaction, and can enhance the SOC between the ground state and the excited state, thereby improving the maximum external quantum efficiency (EQE) of the OLED device. max ), which is conducive to the preparation of high-performance narrow-emission blue-violet OLED devices. In addition, because the polyimide derived from the diamine monoboron compound has a large rigid side group and polymer free volume, it inhibits the formation of charge transfer complexes in the molecular chain, thereby improving the dielectric and optical properties of the flexible substrate, thereby improving the performance of the entire flexible OLED device.
[0034] Specifically, the present invention can achieve the following beneficial effects:
[0035] (1) The present invention develops a new MR-TADF luminescent molecular system by peripherally modifying the strong donor group amino group in the multi-resonance mother core. While maintaining the narrow luminescence spectrum characteristics, the strong N-π-B structure is used to effectively weaken the electron-withdrawing ability of the B atom, thereby causing the light color to be significantly blue-shifted, thereby solving the problem of the scarcity of narrow-emission blue-violet MR-TADF materials at this stage.
[0036] (2) The diamine monoboron compound described in the present invention has LRCT / SRCT interaction, which is beneficial to enhance spin-orbit coupling. When applied to the light-emitting layer of an organic electroluminescent device, it can further improve the device performance and is beneficial to the preparation of a blue-violet narrow emission OLED device with high efficiency and low driving voltage. As illustrated in the embodiments below, the present invention greatly improves the EQE and the light color of the blue-violet light on the basis of narrow emission.
[0037] (3) The polyimide derived from the diamine monoboron compound described in the present invention has extremely rigid large-volume side groups. When applied to the flexible substrate in the organic electroluminescent device, it can enhance the free volume of the substrate film and weaken the generation of charge transfer complexes, thereby making the polyimide film described in the present invention have a low dielectric constant, dielectric loss and excellent optical properties.
[0038] (4) Furthermore, the material obtained by the present invention can be used for both the light-emitting layer and the flexible substrate (as described later) Figure 5 This is the first report.
[0039] The present invention develops a new MR-TADF diamine monoboron compound with a strong donor group amino as the core. The diamine monoboron compound has a long-range charge transfer state, improves the orbital spin coupling constant between the ground state and the excited state, and is helpful for preparing high-performance blue-violet narrow emission OLED devices; the polyimide polymer derived from the diamine monoboron compound has a large rigid side group and free volume, which is conducive to inhibiting the formation of charge transfer complexes, and is helpful for preparing a flexible OLED substrate with high transparency and excellent dielectric properties. In summary, the diamine monoboron compound and its derived polyimide polymer in the present invention have great scientific and technological value and industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 Schematic diagram of the structure of an electroluminescent device.
[0041] Figure 2 The external quantum efficiency-current density relationship characteristic curves of device embodiments 1 to 5 are shown.
[0042] Figure 3It is a driving voltage comparison diagram of device embodiments 1 to 5 and device comparative example 1.
[0043] Figure 4 It is a comparison chart of the dielectric properties of film embodiments 1, 9, 12, 15 and film comparison example 1.
[0044] Figure 5 The schematic diagram is a schematic diagram of the application of the diamine monoboron compound and its derivative polymer in the present invention to an electroluminescent device. DETAILED DESCRIPTION
[0045] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0046] In general, the diamine monoboron compound in the present invention has a general structure as shown in at least one of the general formulas A-1 to A-4; the polyimide derived from the diamine monoboron compound has a general structure as shown in at least one of the general formulas B-1 to B-4:
[0047]
[0048] wherein R1 and R2 are independently selected from hydrogen, deuterium, methyl, phenyl, methoxy, trifluoromethyl, tert-butyl, naphthyl, anthracenyl, silane, halogen, pyrazine, pyridine, pyrimidine, benzimidazole ring, carbazole, indolecarbazole, phenoxazine, phenothiazine, phenoselenazine, phenanthroimidazole, substituted or unsubstituted C2 to C 10 Straight chain alkyl, substituted or unsubstituted C2~C 10 Branched alkyl, substituted or unsubstituted C7~C 30 Aryl, substituted or unsubstituted C2~C 10 Alkoxy, substituted or unsubstituted C1~C 10 Alkylamino, substituted or unsubstituted C2~C 10 In the group consisting of silane groups; Ar is a tetravalent aromatic group; and n=1 to 1000.
[0049] The synthetic routes of general formula A-1 to general formula A-4 are as follows:
[0050]
[0051] Taking general formula A-1 to general formula A-4 as examples, 144 diamine monoboron compounds with specific structures can be obtained, among which:
[0052] In Formulae 1 to 48, R1 is selected from hydrogen, methyl, tert-butyl, benzene ring, methyl, pyridine, pyrimidine, pyrazine, halogen, and R2 is hydrogen;
[0053] In Formula 49 to Formula 60, R1 is hydrogen, and R2 is selected from methyl, trifluoromethyl, and halogen;
[0054] In Formulae 61 to 144, R1 is selected from methyl, tert-butyl, trifluoromethyl, and halogen, and R2 is selected from methyl, trifluoromethyl, and halogen.
[0055] The following is a synthesis example:
[0056] Synthesis Example 1
[0057] The diamine monoboron compound 1 of the present invention conforms to the general formula A-1 and has the following structure:
[0058]
[0059] The preparation method comprises the following steps:
[0060]
[0061] (1) Weigh 10.00 g (36.64 mmol) of 3,5-dichloroiodobenzene, 9.97 g (38.48 mmol) of 4,4'-dinitrodiphenylamine, 15.19 g (109.93 mmol) of potassium carbonate, 0.70 g (3.66 mmol) of cuprous iodide and 0.84 g (7.33 mmol) of L-proline into a 500 mL three-necked flask, and add 80 mL of ultra-dry DMF. Reflux the reaction system at 150°C for 24 hours under magnetic stirring and nitrogen flow at room temperature. After stopping the reaction, the reaction system is cooled to room temperature naturally, and the organic phase and the aqueous phase are separated by extraction with dichloromethane and saturated brine, and the solvent is removed by rotary evaporation. The crude product is chromatographed on a silica gel column using petroleum ether / dichloromethane (15:1 volume ratio) and dried to obtain 12.04 g of a yellow powder.
[0062]
[0063] (2) Weigh 10.00 g (24.74 mmol) of the first step product, 8.79 g (51.95 mmol) of diphenylamine, 1.13 g (1.24 mmol) of tridibenzylideneacetone dipalladium, 0.72 g (2.47 mmol) of tri-tert-butylphosphine tetrafluoroborate, and 14.27 g (148.44 mmol) of sodium tert-butoxide into a 500 mL three-necked flask, and add 60 mL of dry toluene. Then, nitrogen was introduced for 15 minutes, and the mixture was heated to 120° C. and refluxed under nitrogen atmosphere for 20 hours. After the reaction was complete, the mixture was cooled to room temperature, and the organic layer was extracted with dichloromethane and saturated brine, dried, and concentrated. The crude product was chromatographed on a silica gel column using petroleum ether / dichloromethane (15:1 volume ratio), and dried to obtain 14.33 g of yellow powder.
[0064]
[0065] (3) Under nitrogen protection, 10 g (14.93 mmol) of the second step product and o-dichlorobenzene (80 mL) were added to a 500 mL three-necked round-bottom flask in sequence and stirred evenly. Subsequently, 11.51 ml (119.44 mmol) of boron tribromide was added to the above mixed solution, and the temperature was raised to 180°C after the addition was completed. After stirring at 180°C for 24 hours, the reaction was cooled to room temperature, and 39.00 mL (223.95 mmol) of N,N-diisopropylethylamine was added at 0°C. After stirring for half an hour, sodium acetate aqueous solution was added to adjust the pH to neutral, the organic layer was extracted with dichloromethane, dried with magnesium sulfate, concentrated in vacuo, and the o-dichlorobenzene solvent was removed by reduced pressure distillation at 100°C, and column chromatography was performed to obtain 7.11 g of bright yellow powder.
[0066]
[0067] (4) Weigh 7.00 g (10.33 mmol) of the product of the third step and 1.40 g of palladium carbon, place in a 500 mL three-necked flask, keep under a nitrogen atmosphere, add 50 mL of ultra-dry THF, stir and heat to 68 ° C under a nitrogen atmosphere, then slowly add 4.4 mL of hydrazine hydrate to the reaction system, and react for 12 hours after the addition is completed. After stopping the reaction, the reaction system is naturally cooled to room temperature, the palladium carbon is removed by suction filtration, and then the solvent is removed by rotary evaporation. The crude product is chromatographed on a silica gel column with petroleum ether / ethyl acetate (8:1 volume ratio). Dry to obtain a bright yellow solid with a yield of 75%.
[0068] The characterization results of the diamine monoboron derivatives are as follows: mass spectrum is 617.28; NMR results are as follows: 1H NMR(500MHz,Chloroform-d)δ7.44-7.33(m,4H),7.30-7.23(m,1H),7.13-7.07(m,2H),7.09-7.02(m,3H),7. 00(dd,J=6.7,1.4Hz,1H),6.66-6.59(m,2H),6.57-6.51(m,1H),4.00(d,J=5.7Hz,1H),3.94(d,J=5.7Hz,1H).
[0069] Synthesis Example 2
[0070] The diamine monoboron compound 2 of the present invention conforms to the general formula A-2 and has the following structure:
[0071]
[0072] The preparation method comprises the following steps:
[0073]
[0074] (1) 1,3-Dibromo-5-chlorobenzene (5.00 g, 18.49 mmol), diphenylamine (6.57 g, 38.84 mmol), sodium tert-butoxide (10.66 g, 110.97 mmol), tri-tert-butylphosphine tetrafluoroborate (0.54 g, 1.85 mmol), tri(dibenzylideneacetone)dipalladium (0.85 g, 0.93 mmol) and toluene (60 mL) were added into a 250 mL three-necked round-bottom flask in sequence and reacted at 120 °C for 20 hours under a nitrogen atmosphere. After cooling to room temperature, the reaction solution was repeatedly extracted with deionized water and dichloromethane. The crude product was collected and purified on a silica gel column using petroleum ether (PE) / dichloromethane (DCM) as the eluent. The purified product was a white powder with a yield of 80%.
[0075]
[0076] (2) Under nitrogen protection, the first step product (4.00 g, 8.95 mmol) and o-dichlorobenzene (40 mL) were added to a 250 mL three-necked round-bottom flask in sequence and stirred evenly. Subsequently, boron tribromide (3.45 ml, 35.80 mmol) was added to the above mixed solution, and after the addition was completed, the mixture was reacted at 180° C. for 24 hours. Subsequently, the reaction was cooled to room temperature, N,N-diisopropylethylamine (23.38 mL, 134.23 mmol) was added at 0° C., and after stirring for half an hour, sodium acetate aqueous solution was added to adjust the pH to neutral, the organic layer was extracted with dichloromethane, dried with magnesium sulfate, and concentrated in vacuo, and the o-dichlorobenzene solvent was removed by reduced pressure distillation at 100° C., and a bright yellow solid product was obtained by column chromatography, and the reaction yield was 50%.
[0077]
[0078] (3) Weigh 5.00 g (10.99 mmol) of the second step product, 2.38 g (12.09 mmol) of 3,6-diaminocarbazole, and 4.56 g (32.98 mmol) of potassium carbonate, place in a 500 mL three-necked flask, keep under a nitrogen atmosphere, add 50 mL of ultra-dry DMF, stir and heat to 150 ° C under a nitrogen atmosphere and react for 20 h. After stopping the reaction, the reaction system is naturally cooled to room temperature, and the organic phase and the aqueous phase are separated by extraction with dichloromethane and water, and the solvent is removed by rotary evaporation. The crude product is chromatographed on a silica gel column with petroleum ether / ethyl acetate (8:1 volume ratio). Dry to obtain a bright yellow solid with a yield of 87%.
[0079] The characterization results of the diamine monoboron derivatives are as follows: mass spectrum is 615.26; NMR results are as follows: 1 H NMR(500MHz,Chloroform-d)δ7.61(d,J=7.8Hz,1H),7.47-7.33(m,5H),7.26(td,J=7.0,1 .5Hz,1H),7.09-7.02(m,3H),7.05-6.98(m,1H),6.72(dd,J=7.8,2.0Hz,1H),4.26(s,2H).
[0080] Synthesis Example 3
[0081] The diamine monoboron compound 3 of the present invention conforms to the general formula A-3 and has the following structure:
[0082]
[0083] The preparation method comprises the following steps:
[0084]
[0085] (1) 11.68 g (36.64 mmol) of 2-bromo-1,3-difluoro-5-iodobenzene, 9.97 g (38.48 mmol) of 4,4'-dinitrodiphenylamine, 15.19 g (109.93 mmol) of potassium carbonate, 0.70 g (3.66 mmol) of cuprous iodide, 0.84 g (7.33 mmol) of L-proline and 80 mL of ultra-dry DMF were added to a 500 mL three-necked round-bottom flask. Then, under nitrogen protection, the mixed solution was heated to 150°C and stirred for 20 hours. After the reaction was completed, the temperature naturally dropped to room temperature, and toluene was removed by a rotary evaporator. Then, the reaction solution was extracted with dichloromethane and saturated brine, and the organic phase containing the product was collected. The product was separated and purified by column chromatography on a silica gel column using petroleum ether / dichloromethane (15:1 volume ratio) as eluent to finally obtain a yellow solid crystal with a yield of 90%.
[0086]
[0087] (2) Weigh 10.00 g (22.21 mmol) of the first step product, 3.71 g (44.42 mmol) of carbazole, 9.21 g (66.63 mmol) of potassium carbonate and 50 mL of ultra-dry DMF into a three-necked flask. Then, heat the reaction system to 150°C under reflux in a nitrogen environment and stir to react for 20 hours. After the reaction is complete, cool to room temperature, extract with dichloromethane and saturated brine to collect the organic layer, dry and concentrate, and the crude product is chromatographed on a silica gel column using petroleum ether / dichloromethane (10:1 volume ratio) and dried to obtain a yellow powder with a yield of 91%.
[0088]
[0089] (3) Weigh 5 g (6.72 mmol) of the product of the second step above, add it to a 250 ml three-necked round-bottom flask, and add 100 ml of tert-butylbenzene solution thereto, then evacuate the nitrogen, then place the three-necked flask in a low-temperature reaction bath (-40°C), exhaust the air in the needle, extract tert-butyl lithium (19.00 ml, 25.20 mmol) under nitrogen atmosphere protection, then slowly inject it into the flask, and stir thoroughly for 2 h; then heat to room temperature, evacuate again, and remove the n-pentane in the tert-butyl lithium solvent; then slowly add boron tribromide (2.40 ml, 25.20 mmol) at -40°C, keep stirring at room temperature for 1 h; then inject N,N-diisopropylethylamine (7.00 ml, 50.40 mol), heat to 140°C, adjust the condensed water to keep the reaction reflux rate appropriate, and continue to stir the reaction for 12 h. After the reaction is completed, the reaction system is returned to room temperature, ethanol is used to quench the reaction system, the tert-butylbenzene solvent is spin-dried, an appropriate amount of silica gel is added to mix the sample, and the crude product is separated by column chromatography using petroleum ether / dichloromethane (10:1 volume ratio) as eluent to obtain a yellow solid with a yield of 37%.
[0090]
[0091] (4) Add 6.43 g (9.54 mmol) of the product of the third step, 1.40 g of palladium carbon and 50 mL of ultra-dry THF into a 500 mL three-necked flask, stir and heat to 68 ° C under a nitrogen atmosphere, then slowly add 4.2 mL of hydrazine hydrate to the reaction system, and react for 18 hours after the addition is complete. After the reaction is complete, the reaction system is naturally cooled to room temperature, the palladium carbon is removed by suction, and then the solvent is removed by rotary evaporation. The crude product is chromatographed on a silica gel column using petroleum ether / ethyl acetate (10:1 volume ratio). Dry to obtain a bright yellow solid with a yield of 80%.
[0092] The characterization results of the diamine monoboron derivatives are as follows: mass spectrum is 613.24; NMR results are as follows: 1 H NMR(500MHz,Chloroform-d)δ8.18(dd,J=6.2,1.1Hz,1H),8.15-8.09(m,2H),7.68(dd,J=6.3,1.4Hz,1H),7.39(ddd,J=7.4,6.4,1.2Hz,1H),7.33(t,J=6.1 Hz,1H),7.27(ddd,J=8.3,7.1,1.2Hz,1H),7.14(dd,J=19.8,2.0Hz,1H),7.12 -7.07(m,2H),6.66-6.59(m,2H),4.00(d,J=5.7Hz,1H),3.94(d,J=5.7Hz,1H).
[0093] Synthesis Example 4
[0094] The diamine monoboron compound 4 of the present invention conforms to the general formula A-4 and has the following structure:
[0095]
[0096] The preparation method comprises the following steps:
[0097]
[0098] (1) Under nitrogen atmosphere, 5.00 g (22.21 mmol) of 2-bromo-5-chloro-1,3-difluorobenzene, 3.71 g (44.42 mmol) of carbazole, 9.21 g (66.63 mmol) of potassium carbonate and 50 mL of ultra-dry DMF were added to a 250 mL three-necked round-bottom flask, and the temperature was raised to 150 °C for 20 hours. After the reaction was completed, the reaction solution was repeatedly extracted with deionized water and dichloromethane. The crude product was collected and purified on a silica gel column using petroleum ether (PE) as the eluent. The purified product was a white powder with a yield of 88%.
[0099]
[0100] (2) Weigh 3.50 g (6.72 mmol) of the first step product and add it to a 250 ml three-necked round-bottom flask, add 100 ml of tert-butylbenzene solution, then evacuate the nitrogen, then place the three-necked flask in a low-temperature reaction bath (-40°C), exhaust the air in the needle, extract tert-butyl lithium (19.00 ml, 25.20 mmol) under nitrogen atmosphere, then slowly inject it into the flask and stir thoroughly for 2 h; then heat to room temperature, evacuate again to remove the n-pentane in the tert-butyl lithium solvent; then slowly add boron tribromide (2.40 ml, 25.20 mmol) at -40°C, keep stirring at room temperature for 1 h; then inject N,N-diisopropylethylamine (7.00 ml, 50.40 mol), heat to 140°C, adjust the condensed water to keep the reaction reflux rate appropriate, and continue stirring the reaction for 12 h. After the reaction was completed, the reaction system was allowed to return to room temperature, ethanol was used to quench the reaction system, the tert-butylbenzene solvent was spin-dried, an appropriate amount of silica gel was added to mix the sample, and the crude product was separated by column chromatography using petroleum ether as an eluent to obtain a yellow solid with a yield of 41%.
[0101]
[0102] (3) Weigh 4.41 g (9.79 mmol) of the second step product, 2.12 g (10.76 mmol) of 3,6-diaminocarbazole, and 4.56 g (32.98 mmol) of potassium carbonate, place in a 500 mL three-necked flask, keep under a nitrogen atmosphere, add 50 mL of ultra-dry DMF, stir and heat to 150 ° C under a nitrogen atmosphere and react for 20 h. After stopping the reaction, the reaction system is naturally cooled to room temperature, and the organic phase and the aqueous phase are separated by extraction with dichloromethane and water, and the solvent is removed by rotary evaporation. The crude product is chromatographed on a silica gel column with petroleum ether / ethyl acetate (15:1 volume ratio). Dry to obtain a bright yellow solid with a yield of 77%.
[0103] The characterization results of the diamine monoboron derivatives are as follows: mass spectrum is 611.23; NMR results are as follows: 1 H NMR(500MHz,Chloroform-d)δ8.18(dd,J=6.2,1.1Hz,1H),8.15-8.09(m,2H),7.68(dd,J=6.3,1.4Hz,1H),7.64-7.58(m,2H),7.45(d,J=2.0H z,1H),7.39(ddd,J=7.4,6.4,1.2Hz,1H),7.33(t,J=6.1Hz,1H),7.27(ddd,J=8.3,7.2,1.2Hz,1H),6.72(dd,J=7.7,2.0Hz,1H),4.26(s,2H).
[0104] Synthesis Example 5
[0105] The diamine monoboron compound 13 of the present invention conforms to the general formula A-1 and has the following structure:
[0106]
[0107] The preparation method comprises the following steps:
[0108]
[0109] (1) Weigh 10.00 g (36.64 mmol) of 3,5-dichloroiodobenzene, 9.97 g (38.48 mmol) of 4,4'-dinitrodiphenylamine, 15.19 g (109.93 mmol) of potassium carbonate, 0.70 g (3.66 mmol) of cuprous iodide and 0.84 g (7.33 mmol) of L-proline into a 500 mL three-necked flask, and add 80 mL of ultra-dry DMF. Reflux the reaction system at 150°C for 24 hours under magnetic stirring and nitrogen flow at room temperature. After stopping the reaction, the reaction system is cooled to room temperature naturally, and the organic phase and the aqueous phase are separated by extraction with dichloromethane and saturated brine, and the solvent is removed by rotary evaporation. The crude product is chromatographed on a silica gel column using petroleum ether / dichloromethane (15:1 volume ratio) and dried to obtain 12.04 g of a yellow powder.
[0110]
[0111] (2) Weigh 10.00 g (23.75 mmol) of di(4-iodophenyl)amine, 6.08 g (49.88 mmol) of phenylboronic acid, 19.69 g (142.50 mmol) of potassium carbonate and 1.65 g (1.43 mmol) of tetrakistriphenylphosphine palladium into a 500 mL three-necked flask, and add 60 mL of toluene, 20 mL of ethanol and 20 mL of water. Reflux the reaction system at 110° C. for 24 hours under magnetic stirring and nitrogen flow at room temperature. After stopping the reaction, the reaction system is cooled to room temperature naturally, and the organic phase and the aqueous phase are separated by extraction with dichloromethane and saturated brine, and the solvent is removed by rotary evaporation. The crude product is chromatographed on a silica gel column using petroleum ether / dichloromethane (15:1 volume ratio) and dried to obtain a white powder.
[0112]
[0113] (3) Weigh 10.00 g (24.74 mmol) of the first step product, 16.70 g (51.95 mmol) of the second step product, 1.13 g (1.24 mmol) of tridibenzylideneacetone dipalladium, 0.72 g (2.47 mmol) of tri-tert-butylphosphine tetrafluoroborate, and 14.27 g (148.44 mmol) of sodium tert-butoxide into a 500 mL three-necked flask, and add 60 mL of dry toluene. Then, nitrogen was introduced for 15 minutes, and the mixture was heated to 120° C. and refluxed under nitrogen atmosphere for 20 hours. After the reaction was complete, the mixture was cooled to room temperature, and the organic layer was extracted with dichloromethane and saturated brine, dried, and concentrated. The crude product was chromatographed on a silica gel column using petroleum ether / dichloromethane (15:1 volume ratio) and dried to obtain a yellow powder.
[0114]
[0115] (4) Under nitrogen protection, 10 g (10.27 mmol) of the third step product and o-dichlorobenzene (80 mL) were added to a 500 mL three-necked round-bottom flask in sequence and stirred evenly. Subsequently, 7.97 ml (82.72 mmol) of boron tribromide was added to the above mixed solution, and the temperature was raised to 180°C after the addition was completed. After stirring at 180°C for 24 hours, the reaction was cooled to room temperature, and 26.82 mL (154.05 mmol) of N,N-diisopropylethylamine was added at 0°C. After stirring for half an hour, sodium acetate aqueous solution was added to adjust the pH to neutral, the organic layer was extracted with dichloromethane, dried with magnesium sulfate, concentrated in vacuo, and the o-dichlorobenzene solvent was removed by reduced pressure distillation at 100°C, and column chromatography was performed to obtain 6.27 g of bright yellow powder.
[0116]
[0117] (5) Weigh 10.14 g (10.33 mmol) of the product of the fourth step and 1.40 g of palladium carbon, place in a 500 mL three-necked flask, keep under a nitrogen atmosphere, add 50 mL of ultra-dry THF, stir and heat to 68 ° C under a nitrogen atmosphere, then slowly add 4.4 mL of hydrazine hydrate to the reaction system, and react for 12 hours after the addition is completed. After stopping the reaction, the reaction system is naturally cooled to room temperature, the palladium carbon is removed by suction filtration, and then the solvent is removed by rotary evaporation. The crude product is chromatographed on a silica gel column with petroleum ether / ethyl acetate (8:1 volume ratio). Dry to obtain a bright yellow solid with a yield of 67%.
[0118] The characterization results of the diamine monoboron derivatives are as follows: mass spectrum is 921.40; NMR results are as follows: 1 H NMR(500MHz,Chloroform-d)δ7.67-7.52(m,8H),7.44(ddt,J=7.7,6.2,1.3Hz,4H),7.44-7.36(m,2H), 7.17-7.07(m,5H),6.66-6.59(m,2H),6.57-6.51(m,1H),4.00(d,J=5.7Hz,1H),3.94(d,J=5.7Hz,1H).
[0119] Synthesis Example 6
[0120] The diamine monoboron compound 49 of the present invention conforms to the general formula A-1 and has the following structure:
[0121]
[0122] The preparation method comprises the following steps:
[0123]
[0124] (1) Weigh 10.00 g (36.64 mmol) of 3,5-dichloroiodobenzene, 9.97 g (38.48 mmol) of 4,4'-dinitrodiphenylamine, 15.19 g (109.93 mmol) of potassium carbonate, 0.70 g (3.66 mmol) of cuprous iodide and 0.84 g (7.33 mmol) of L-proline into a 500 mL three-necked flask, and add 80 mL of ultra-dry DMF. Reflux the reaction system at 150°C for 24 hours under magnetic stirring and nitrogen flow at room temperature. After stopping the reaction, the reaction system is cooled to room temperature naturally, and the organic phase and the aqueous phase are separated by extraction with dichloromethane and saturated brine, and the solvent is removed by rotary evaporation. The crude product is chromatographed on a silica gel column using petroleum ether / dichloromethane (15:1 volume ratio) and dried to obtain 12.04 g of a yellow powder.
[0125]
[0126] (2) Weigh 10.00 g (82.52 mmol) of 2,6-dimethylaniline, 12.96 g (82.52 mmol) of bromobenzene, 3.78 g (4.13 mmol) of tridibenzylideneacetone dipalladium, 2.40 g (8.26 mmol) of tri-tert-butylphosphine tetrafluoroborate, and 23.79 g (247.56 mmol) of sodium tert-butoxide into a 500 mL three-necked flask, and add 60 mL of dry toluene. Then, nitrogen was introduced for 15 minutes, and the mixture was heated to 120° C. and refluxed under nitrogen atmosphere for 22 hours. After the reaction was complete, the mixture was cooled to room temperature, and the organic layer was extracted with dichloromethane and saturated brine, dried, and concentrated. The crude product was chromatographed on a silica gel column using petroleum ether / dichloromethane (20:1 volume ratio) and dried to obtain 18.75 g of white powder.
[0127]
[0128] (3) Weigh 10.00 g (24.74 mmol) of the first step product, 10.25 g (51.95 mmol) of the second step product, 1.13 g (1.24 mmol) of tridibenzylideneacetone dipalladium, 0.72 g (2.47 mmol) of tri-tert-butylphosphine tetrafluoroborate, and 14.27 g (148.44 mmol) of sodium tert-butoxide into a 500 mL three-necked flask, and add 60 mL of dry toluene. Then, nitrogen was introduced for 15 minutes, and the mixture was heated to 120° C. and refluxed under nitrogen atmosphere for 20 hours. After the reaction was complete, the mixture was cooled to room temperature, and the organic layer was extracted with dichloromethane and saturated brine, dried, and concentrated. The crude product was chromatographed on a silica gel column using petroleum ether / dichloromethane (15:1 volume ratio) and dried to obtain a yellow powder.
[0129]
[0130] (4) Under nitrogen protection, 7.45 g (10.27 mmol) of the product of the third step and o-dichlorobenzene (80 mL) were added to a 500 mL three-necked round-bottom flask in sequence and stirred evenly. Subsequently, 7.97 ml (82.72 mmol) of boron tribromide was added to the above mixed solution, and the temperature was raised to 180°C after the addition was completed. After stirring at 180°C for 24 hours, the reaction was cooled to room temperature, and 26.82 mL (154.05 mmol) of N,N-diisopropylethylamine was added at 0°C. After stirring for half an hour, sodium acetate aqueous solution was added to adjust the pH to neutral, the organic layer was extracted with dichloromethane, dried with magnesium sulfate, concentrated in vacuo, and the o-dichlorobenzene solvent was removed by reduced pressure distillation at 100°C, and column chromatography was performed to obtain a bright yellow powder.
[0131]
[0132] (5) Weigh 7.56 g (10.33 mmol) of the product of the fourth step and 1.40 g of palladium carbon, place in a 500 mL three-necked flask, keep under a nitrogen atmosphere, add 50 mL of ultra-dry THF, stir and heat to 68 ° C under a nitrogen atmosphere, then slowly add 4.4 mL of hydrazine hydrate to the reaction system, and react for 12 hours after the addition is completed. After stopping the reaction, the reaction system is naturally cooled to room temperature, the palladium carbon is removed by suction filtration, and then the solvent is removed by rotary evaporation. The crude product is chromatographed on a silica gel column with petroleum ether / ethyl acetate (8:1 volume ratio). Dry to obtain a bright yellow solid with a yield of 71%.
[0133] The characterization results of the diamine monoboron derivatives are as follows: mass spectrum is 673.34; NMR results are as follows: 1 H NMR(500MHz,Chloroform-d)δ7.38(dd,J=7.3,1.4Hz,1H),7.26(td,J=7.0,1.4Hz,1H),7.13(dd,J=6.8,1.5Hz,1H),7.14-7 .07(m,5H),7.05(td,J=7.3,1.5Hz,1H),6.71-6.65(m,1H),6.65-6.59(m,2H),4.00(d,J=5.7Hz,1H),3.94(d,J=5.7Hz,1H).
[0134] Similarly, the remaining diamine monoboron compounds can be synthesized similarly.
[0135] The above-mentioned diamine monoboron compound can be used in an organic electroluminescent device. For example, the diamine monoboron compound can be used as a luminescent guest material of a luminescent layer in an organic electroluminescent device. Figure 1The schematic diagram of the structure of an electroluminescent device is shown as an example. The organic electroluminescent device obtained accordingly comprises a counter electrode and a transmission layer, a light-emitting layer and an injection layer between the counter electrodes, wherein the light-emitting layer contains the diamine monoboron compound of the present invention.
[0136] The diamine monoboron compound described in the present invention can be used as a guest luminescent material in OLED electroluminescent devices. Taking the use of ITO substrate as an example, the specific device preparation process may include: substrate pretreatment, ultrasonic cleaning of the ITO (indium tin oxide) glass substrate in ITO cleaning agent, isopropyl alcohol, acetone, ethanol, and deionized water for 30 minutes, drying in an oven at 120°C for 2 hours after drying with dry nitrogen. Before preparing the device, the ITO glass substrate is surface treated with oxygen plasma for 5 minutes, and then transferred to an organic vacuum chamber for evaporation of organic functional layer materials. After completion, it is vacuum transferred to a metal vacuum chamber for evaporation of metal electrodes. In the specific preparation process, the best host material, exciton blocking layer material or injection transport layer material can be selected according to the properties of the diamine monoboron compound itself, such as the luminescence peak position, the lowest singlet and triplet energy level values; in addition, the film thickness of each functional layer and the concentration of host and guest doping are also systematically optimized.
[0137] The following is a device embodiment (each organic functional layer is optimized):
[0138] Device Comparison Example 1:
[0139] ITO / MoO3(10nm) / TAPC(60nm) / mCP(10nm) / PPF: Dopant(9wt%, 20nm) / PPF(10nm) / TmPyPB(30nm) / LiF(1nm) / Al(100nm).
[0140] The guest luminescent material (Dopant) of the luminescent layer is a conventional MR-TADF monoboron compound PAB. The device has an electroluminescent peak wavelength of 452nm, a half-peak width (FWHM) of 28nm, a maximum external quantum efficiency (EQEmax) of 21.6%, a driving voltage of 4.0V, and a device life LT95 of 75 hours @ initial brightness 2000cd / m 2 .
[0141] Device Example 1:
[0142] ITO / MoO3(10nm) / TAPC(60nm) / mCP(10nm) / PPF: Dopant(9wt%, 20nm) / PPF(10nm) / TmPyPB(30nm) / LiF(1nm) / Al(100nm).
[0143] The guest luminescent material (Dopant) of the luminescent layer is the diamine monoboron compound 1 described in the present invention. The device has an electroluminescent peak wavelength of 417 nm, a half-peak width (FWHM) of 27 nm, a maximum external quantum efficiency (EQEmax) of 32.9%, a driving voltage of 3.4 V, and a device life LT95 of 90 hours @ initial brightness 2000 cd / m 2 .
[0144] Device Example 2:
[0145] ITO / MoO3(10nm) / TAPC(60nm) / mCP(10nm) / PPF: Dopant(9wt%, 20nm) / PPF(10nm) / TmPyPB(30nm) / LiF(1nm) / Al(100nm).
[0146] The guest luminescent material (Dopant) of the luminescent layer is the diamine monoboron compound 2 described in the present invention. The device has an electroluminescent peak wavelength of 425nm, a half-peak width (FWHM) of 24nm, a maximum external quantum efficiency (EQEmax) of 30.7%, a driving voltage of 3.4V, and a device life LT95 of 95 hours @ initial brightness 2000cd / m 2 .
[0147] Device Example 3:
[0148] ITO / MoO3(10nm) / TAPC(60nm) / mCP(10nm) / PPF: Dopant(6wt%, 20nm) / PPF(10nm) / TmPyPB(30nm) / LiF(1nm) / Al(100nm).
[0149] The guest luminescent material (Dopant) of the luminescent layer is the diamine monoboron compound 3 described in the present invention. The device has an electroluminescent peak wavelength of 420nm, a half-peak width (FWHM) of 25nm, a maximum external quantum efficiency (EQEmax) of 33.4%, a driving voltage of 3.5V, and a device life LT95 of 92 hours @ initial brightness 2000cd / m 2 .
[0150] Device Example 4:
[0151] ITO / MoO3(10nm) / TAPC(60nm) / mCP(10nm) / PPF: Dopant(6wt%, 20nm) / PPF(10nm) / TmPyPB(30nm) / LiF(1nm) / Al(100nm).
[0152] The guest luminescent material (Dopant) of the luminescent layer is the diamine monoboron compound 4 described in the present invention. The device has an electroluminescent peak wavelength of 426 nm, a half-peak width (FWHM) of 26 nm, a maximum external quantum efficiency (EQEmax) of 34.1%, a driving voltage of 3.5 V, and a device life LT95 of 100 hours @ initial brightness 2000 cd / m 2 .
[0153] Device Example 5:
[0154] ITO / MoO3(10nm) / TAPC(60nm) / mCP(10nm) / PPF: Dopant(6wt%, 20nm) / PPF(10nm) / TmPyPB(30nm) / LiF(1nm) / Al(100nm).
[0155] The guest luminescent material (Dopant) of the luminescent layer is the diamine monoboron compound 5 described in the present invention. The device has an electroluminescent peak wavelength of 429 nm, a half-peak width (FWHM) of 26 nm, a maximum external quantum efficiency (EQEmax) of 32.9%, a driving voltage of 3.4 V, and a device life LT95 of 98 hours @ initial brightness 2000 cd / m 2 .
[0156] Device Example 6:
[0157] ITO / MoO3(10nm) / TAPC(60nm) / mCP(10nm) / PPF: Dopant(6wt%, 20nm) / PPF(10nm) / TmPyPB(30nm) / LiF(1nm) / Al(100nm).
[0158] The guest luminescent material (Dopant) of the luminescent layer is the diamine monoboron compound 6 described in the present invention. The device has an electroluminescent peak wavelength of 429 nm, a half-peak width (FWHM) of 26 nm, a maximum external quantum efficiency (EQEmax) of 35.1%, a driving voltage of 3.4 V, and a device life LT95 of 100 hours @ initial brightness 2000 cd / m 2 .
[0159] Device Example 7:
[0160] ITO / MoO3(10nm) / TAPC(60nm) / mCP(10nm) / PPF: Dopant(9wt%, 20nm) / PPF(10nm) / TmPyPB(30nm) / LiF(1nm) / Al(100nm).
[0161] The guest luminescent material (Dopant) of the luminescent layer is the diamine monoboron compound 7 described in the present invention. The device has an electroluminescent peak wavelength of 429 nm, a half-peak width (FWHM) of 28 nm, a maximum external quantum efficiency (EQEmax) of 34.3%, a driving voltage of 3.4 V, and a device life LT95 of 89 hours @ initial brightness 2000 cd / m 2 .
[0162] Device Example 8:
[0163] ITO / MoO3(10nm) / TAPC(60nm) / mCP(10nm) / PPF: Dopant(9wt%, 20nm) / PPF(10nm) / TmPyPB(30nm) / LiF(1nm) / Al(100nm).
[0164] The guest luminescent material (Dopant) of the luminescent layer is the diamine monoboron compound 8 described in the present invention. The device has an electroluminescent peak wavelength of 430 nm, a half-peak width (FWHM) of 28 nm, a maximum external quantum efficiency (EQEmax) of 30.1%, a driving voltage of 3.4 V, and a device life LT95 of 92 hours @ initial brightness 2000 cd / m 2 .
[0165] Device Example 9:
[0166] ITO / MoO3(10nm) / TAPC(60nm) / mCP(10nm) / PPF: Dopant(9wt%, 20nm) / PPF(10nm) / TmPyPB(30nm) / LiF(1nm) / Al(100nm).
[0167] The guest luminescent material (Dopant) of the luminescent layer is the diamine monoboron compound 9 described in the present invention. The device has an electroluminescent peak wavelength of 422nm, a half-peak width (FWHM) of 25nm, a maximum external quantum efficiency (EQEmax) of 34.6%, a driving voltage of 3.3V, and a device life LT95 of 88 hours @ initial brightness 2000cd / m 2 .
[0168] Device Example 10:
[0169] ITO / MoO3(10nm) / TAPC(60nm) / mCP(10nm) / PPF: Dopant(9wt%, 20nm) / PPF(10nm) / TmPyPB(30nm) / LiF(1nm) / Al(100nm).
[0170] The guest luminescent material (Dopant) of the luminescent layer is the diamine monoboron compound 10 described in the present invention. The device has an electroluminescent peak wavelength of 429 nm, a half-peak width (FWHM) of 27 nm, a maximum external quantum efficiency (EQEmax) of 31.8%, a driving voltage of 3.5 V, and a device life LT95 of 91 hours @ initial brightness 2000 cd / m 2 .
[0171] Device Example 11:
[0172] ITO / MoO3(10nm) / TAPC(60nm) / mCP(10nm) / PPF: Dopant(3wt%, 20nm) / PPF(10nm) / TmPyPB(30nm) / LiF(1nm) / Al(100nm).
[0173] The guest luminescent material (Dopant) of the luminescent layer is the diamine monoboron compound 11 described in the present invention. The device has an electroluminescent peak wavelength of 414 nm, a half-peak width (FWHM) of 23 nm, a maximum external quantum efficiency (EQEmax) of 30.9%, a driving voltage of 3.4 V, and a device life LT95 of 80 hours @ initial brightness 2000 cd / m 2 .
[0174] Device Example 12:
[0175] ITO / MoO3(10nm) / TAPC(60nm) / mCP(10nm) / PPF: Dopant(3wt%, 20nm) / PPF(10nm) / TmPyPB(30nm) / LiF(1nm) / Al(100nm).
[0176] The guest luminescent material (Dopant) of the luminescent layer is the diamine monoboron compound 12 described in the present invention. The device has an electroluminescent peak wavelength of 420 nm, a half-peak width (FWHM) of 23 nm, a maximum external quantum efficiency (EQEmax) of 32.0%, a driving voltage of 3.4 V, and a device life LT95 of 85 hours @ initial brightness 2000 cd / m 2 .
[0177] Device Example 13:
[0178] ITO / MoO3(10nm) / TAPC(60nm) / mCP(10nm) / PPF: Dopant(3wt%, 20nm) / PPF(10nm) / TmPyPB(30nm) / LiF(1nm) / Al(100nm).
[0179] The guest luminescent material (Dopant) of the luminescent layer is the diamine monoboron compound 13 described in the present invention. The device has an electroluminescent peak wavelength of 410 nm, a half-peak width (FWHM) of 26 nm, a maximum external quantum efficiency (EQEmax) of 30.1%, a driving voltage of 3.6 V, and a device life LT95 of 80 hours @ initial brightness 2000 cd / m 2 .
[0180] Device Example 14:
[0181] ITO / MoO3(10nm) / TAPC(60nm) / mCP(10nm) / PPF: Dopant(3wt%, 20nm) / PPF(10nm) / TmPyPB(30nm) / LiF(1nm) / Al(100nm).
[0182] The guest luminescent material (Dopant) of the luminescent layer is the diamine monoboron compound 14 described in the present invention. The device has an electroluminescent peak wavelength of 416 nm, a half-peak width (FWHM) of 28 nm, a maximum external quantum efficiency (EQEmax) of 32.4%, a driving voltage of 3.7 V, and a device life LT95 of 78 hours @ initial brightness 2000 cd / m 2 .
[0183] Device Example 15:
[0184] ITO / MoO3(10nm) / TAPC(60nm) / mCP(10nm) / PPF: Dopant(6wt%, 20nm) / PPF(10nm) / TmPyPB(30nm) / LiF(1nm) / Al(100nm).
[0185] The guest luminescent material (Dopant) of the luminescent layer is the diamine monoboron compound 15 described in the present invention. The device has an electroluminescent peak wavelength of 414 nm, a half-peak width (FWHM) of 26 nm, a maximum external quantum efficiency (EQEmax) of 32.3%, a driving voltage of 3.6 V, and a device life LT95 of 88 hours @ initial brightness 2000 cd / m 2 .
[0186] Device Example 16:
[0187] ITO / MoO3(10nm) / TAPC(60nm) / mCP(10nm) / PPF: Dopant(6wt%, 20nm) / PPF(10nm) / TmPyPB(30nm) / LiF(1nm) / Al(100nm).
[0188] The guest luminescent material (Dopant) of the luminescent layer is the diamine monoboron compound 16 described in the present invention. The device has an electroluminescent peak wavelength of 419 nm, a half-peak width (FWHM) of 29 nm, a maximum external quantum efficiency (EQEmax) of 33.0%, a driving voltage of 3.5 V, and a device life LT95 of 90 hours @ initial brightness 2000 cd / m 2 .
[0189] Device Example 17:
[0190] ITO / MoO3(10nm) / TAPC(60nm) / mCP(10nm) / PPF: Dopant(3wt%, 20nm) / PPF(10nm) / TmPyPB(30nm) / LiF(1nm) / Al(100nm).
[0191] The guest luminescent material (Dopant) of the luminescent layer is the diamine monoboron compound 17 described in the present invention. The device has an electroluminescent peak wavelength of 410 nm, a half-peak width (FWHM) of 29 nm, a maximum external quantum efficiency (EQEmax) of 30.7%, a driving voltage of 3.7 V, and a device life LT95 of 85 hours @ initial brightness 2000 cd / m 2 .
[0192] Device Example 18:
[0193] ITO / MoO3(10nm) / TAPC(60nm) / mCP(10nm) / PPF: Dopant(3wt%, 20nm) / PPF(10nm) / TmPyPB(30nm) / LiF(1nm) / Al(100nm).
[0194] The guest luminescent material (Dopant) of the luminescent layer is the diamine monoboron compound 18 described in the present invention. The device has an electroluminescent peak wavelength of 416 nm, a half-peak width (FWHM) of 29 nm, a maximum external quantum efficiency (EQEmax) of 31.1%, a driving voltage of 3.6 V, and a device life LT95 of 90 hours @ initial brightness 2000 cd / m 2 .
[0195] Device Example 19:
[0196] ITO / MoO3(10nm) / TAPC(60nm) / mCP(10nm) / PPF: Dopant(9wt%, 20nm) / PPF(10nm) / TmPyPB(30nm) / LiF(1nm) / Al(100nm).
[0197] The guest luminescent material (Dopant) of the luminescent layer is the diamine monoboron compound 19 described in the present invention. The device has an electroluminescent peak wavelength of 410 nm, a half-peak width (FWHM) of 24 nm, a maximum external quantum efficiency (EQEmax) of 32.0%, a driving voltage of 3.5 V, and a device life LT95 of 94 hours @ initial brightness 2000 cd / m 2 .
[0198] Device Example 20:
[0199] ITO / MoO3(10nm) / TAPC(60nm) / mCP(10nm) / PPF: Dopant(9wt%, 20nm) / PPF(10nm) / TmPyPB(30nm) / LiF(1nm) / Al(100nm).
[0200] The guest luminescent material (Dopant) of the luminescent layer is the diamine monoboron compound 20 described in the present invention. The device has an electroluminescent peak wavelength of 415 nm, a half-peak width (FWHM) of 26 nm, a maximum external quantum efficiency (EQEmax) of 33.9%, a driving voltage of 3.4 V, and a device life LT95 of 100 hours @ initial brightness 2000 cd / m 2 .
[0201] The above examples demonstrate that the diamine monoboron compound based on the present invention has blue-violet light emission (410nm-430nm) and extremely narrow half-peak width (<30nm), which can effectively improve the color purity of the device. In addition, due to the introduction of strong donor amino groups, LRCT / SRCT interactions are generated, and OLED devices prepared based on diamine monoboron derivatives can obtain higher device efficiency (EQE>30%) and lower driving voltage.
[0202] Attached Figure 2 The external quantum efficiency-current density relationship characteristic curves of device embodiments 1 to 5. From the device external quantum efficiency curves, it can be clearly concluded that the luminous efficiency of the material is at a high level, which meets the requirements for the industrial application of organic electroluminescent materials. Figure 3 This is a driving voltage comparison diagram of device embodiments 1 to 5 and device comparison example 1. It can be seen that the OLED device prepared from the diamine monoboron compound described in the present invention has a lower driving voltage than the conventional MR-TADF material, which meets the requirements for industrial application of organic electroluminescent materials.
[0203] According to another aspect of the present invention, the polyimide polymer derived from the diamine monoboron compound of the present invention can be used as a flexible substrate and applied to OLED electroluminescent devices. The specific polyimide film preparation process may include, for example: (1) adding one or more diamines to a polar aprotic organic solvent under the protection of a nitrogen atmosphere at 0-20°C, and then adding one or more dianhydrides twice, with an interval of 10-30 minutes between the two times, and controlling the molar ratio of diamine to dianhydride to be 0.95-1.05, and continuously stirring for 5-24 hours to obtain a polyamic acid (PAA) solution. (2) uniformly coating the polyamic acid solution on a substrate, removing part of the solvent in the polyamic acid solution by soft baking at 80-100°C, and subjecting the polyamic acid solution to thermal imidization, mainly by step-by-step heating, and then cooling to room temperature to obtain a polyimide film.
[0204] The following are examples of thin films:
[0205] Film Comparative Example 1:
[0206] (1) Under nitrogen atmosphere at room temperature, 10 mmol of 4,4'-diaminodiphenyl ether (ODA) was dissolved in ultra-dry N,N-dimethylacetamide (DMAc) in a flask, and then 10 mmol of pyromellitic dianhydride (PMDA) was added twice and stirred for 24 h to obtain a PAA-0 solution.
[0207] (2) Then, the polyamic acid solution was evenly spread on the clean substrate by spin coating at a rotation speed of 1200 rpm for 40 s, and soft-baked on a hot plate at 90° C. for 15 minutes to remove part of the organic solvent.
[0208] (3) Finally, thermal imidization is carried out in a nitrogen atmosphere, mainly by step-heating, the heating program is 100°C / 1 hour, 200°C / 1 hour, 300°C / 1 hour, 350°C / 1 hour, the heating rate is 5°C / minute, and then cooled to room temperature to obtain a polyimide substrate PI-0. The polyimide PI-0 has a Young's modulus of 3.20 GPa, a dielectric constant of 3.2 at 10 GHz, a dielectric loss of 15‰ at 10 GHz, and a transmittance of 50% at 450 nm.
[0209] Film Example 1, conforming to the general formula B-1:
[0210] The difference between the preparation method of Example 1 and Comparative Example 1 is that the diamine in step (1) is replaced by the diamine monoboron compound 1 of the present invention, and the dianhydride is replaced by 4,4'-oxydiphthalic anhydride (ODPA), and the PAA-1 solution is directly polymerized, and then the polyimide PI-1 is obtained by curing at 350° C. The Young's modulus of the polyimide PI-1 is 3.10 Gpa, the dielectric constant is 3.15 at 10 GHz, the dielectric loss is 10.1‰ at 10 GHz, and the transmittance at 450 nm is 88%.
[0211] Film Example 2, conforming to Formula B-1:
[0212] The difference between the preparation method of this embodiment and the film embodiment 1 is that the diamine in step (1) is replaced by a mixed diamine of a diamine monoboron compound 1 and 4,4'-diaminodiphenyl ether (ODA), the mixed molar ratio is 1:9, and PAA-2 is obtained by polymerization, and then polyimide PI-2 is obtained by curing at 350°C. The Young's modulus of the polyimide PI-2 is 3.03 GPa, the dielectric constant is 3.10 at 10 GHz, the dielectric loss is 9.9‰ at 10 GHz, and the transmittance at 450 nm is 88%.
[0213] Film Example 3, conforming to Formula B-1:
[0214] The difference between the preparation method of this embodiment and the film embodiment 1 is that the diamine in step (1) is replaced by a mixed diamine of a diamine monoboron compound 1 and 4,4'-diaminodiphenyl ether (ODA), the mixed molar ratio is 2:8, and PAA-3 is obtained by polymerization, and then polyimide PI-3 is obtained by curing at 350°C. The Young's modulus of the polyimide PI-3 is 3.11 GPa, the dielectric constant is 3.10 at 10 GHz, the dielectric loss is 8.0‰ at 10 GHz, and the transmittance at 450 nm is 87%.
[0215] Film Example 4, conforming to Formula B-1:
[0216] The difference between the preparation method of this embodiment and that of the film embodiment 1 is that the dianhydride in step (1) is replaced with 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), and PAA-13 is directly polymerized, and then the polyimide PI-13 is obtained by curing at 350° C. The Young's modulus of the polyimide PI-13 is 3.19 GPa, the dielectric constant is 2.99 at 10 GHz, the dielectric loss is 6.0‰ at 10 GHz, and the transmittance at 450 nm is 93%.
[0217] Film Example 5, conforming to Formula B-1:
[0218] The difference between the preparation method of this embodiment and that of the film embodiment 1 is that the dianhydride in step (1) is replaced with 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), and PAA-14 is directly polymerized, and then the polyimide PI-14 is obtained by curing at 350° C. The Young's modulus of the polyimide PI-14 is 3.25 GPa, the dielectric constant is 3.00 at 10 GHz, the dielectric loss is 7.1‰ at 10 GHz, and the transmittance at 450 nm is 90%.
[0219] Film Example 6, conforming to Formula B-1:
[0220] The difference between the preparation method of this embodiment and that of the film embodiment 1 is that the dianhydride in step (1) is replaced with pyromellitic dianhydride (PMDA), and PAA-15 is directly polymerized, and then the polyimide PI-15 is obtained by curing at 350° C. The Young's modulus of the polyimide PI-15 is 3.11 GPa, the dielectric constant is 3.09 at 10 GHz, the dielectric loss is 8.5‰ at 10 GHz, and the transmittance at 450 nm is 85%.
[0221] Film Example 7, conforming to Formula B-1:
[0222] The difference between the preparation method of this embodiment and that of the film embodiment 1 is that the dianhydride in step (1) is replaced by bisphenol A diether dianhydride (BPADA), and PAA-16 is directly polymerized, and then polyimide PI-16 is obtained by curing at 350° C. The Young's modulus of the polyimide PI-16 is 3.21 GPa, the dielectric constant is 3.02 at 10 GHz, the dielectric loss is 7.7‰ at 10 GHz, and the transmittance at 450 nm is 91%.
[0223] Film Example 8, conforming to Formula B-1:
[0224] The difference between the preparation method of this embodiment and that of the film embodiment 1 is that the dianhydride in step (1) is replaced with hexafluorodianhydride (6FDA), and PAA-17 is directly polymerized, and then polyimide PI-17 is obtained by curing at 350° C. The Young's modulus of the polyimide PI-17 is 3.38 GPa, the dielectric constant is 2.97 at 10 GHz, the dielectric loss is 6.5‰ at 10 GHz, and the transmittance at 450 nm is 95%.
[0225] Film Example 9, conforming to Formula B-2:
[0226] The difference between the preparation method of this embodiment and the film embodiment 1 is that the diamine in step (1) is replaced by a diamine monoboron compound 2, and PAA-4 is obtained by polymerization, and then polyimide PI-4 is obtained by curing at 350° C. The Young's modulus of the polyimide PI-4 is 3.20 GPa, the dielectric constant is 3.05 at 10 GHz, the dielectric loss is 8.2‰ at 10 GHz, and the transmittance at 450 nm is 89%.
[0227] Film Example 10, conforming to Formula B-2:
[0228] The difference between the preparation method of this embodiment and the film embodiment 1 is that the diamine in step (1) is replaced by a mixed diamine of a diamine monoboron compound 2 and 4,4'-diaminodiphenyl ether (ODA), the mixed molar ratio is 1:9, and PAA-5 is obtained by polymerization, and then polyimide PI-5 is obtained by curing at 350°C. The Young's modulus of the polyimide PI-5 is 3.17 GPa, the dielectric constant is 3.01 at 10 GHz, the dielectric loss is 6.7‰ at 10 GHz, and the transmittance at 450 nm is 95%.
[0229] Film Example 11, conforming to Formula B-2:
[0230] The difference between the preparation method of this embodiment and the film embodiment 1 is that the diamine in step (1) is replaced by a mixed diamine of a diamine monoboron compound 2 and 4,4'-diaminodiphenyl ether (ODA), the mixed molar ratio is 2:8, and PAA-6 is obtained by polymerization, and then polyimide PI-6 is obtained by curing at 350°C. The Young's modulus of the polyimide PI-6 is 3.11 GPa, the dielectric constant is 3.11 at 10 GHz, the dielectric loss is 7.8‰ at 10 GHz, and the transmittance at 450 nm is 91%.
[0231] Film Example 12, conforming to Formula B-3:
[0232] The difference between the preparation method of this embodiment and that of the film embodiment 1 is that the diamine in step (1) is replaced by a diamine monoboron compound 3, and PAA-7 is obtained by polymerization, and then polyimide PI-7 is obtained by curing at 350° C. The Young's modulus of the polyimide PI-7 is 3.20 GPa, the dielectric constant is 3.08 at 10 GHz, the dielectric loss is 6.9‰ at 10 GHz, and the transmittance at 450 nm is 93%.
[0233] Film Example 13, conforming to Formula B-3:
[0234] The difference between the preparation method of this embodiment and the film embodiment 1 is that the diamine in step (1) is replaced by a mixed diamine of a diamine monoboron compound 3 and 4,4'-diaminodiphenyl ether (ODA), the mixed molar ratio is 1:9, and PAA-8 is obtained by polymerization, and then polyimide PI-8 is obtained by curing at 350°C. The Young's modulus of the polyimide PI-8 is 3.09 GPa, the dielectric constant is 3.00 at 10 GHz, the dielectric loss is 6.1‰ at 10 GHz, and the transmittance at 450 nm is 95%.
[0235] Film Example 14, conforming to Formula B-3:
[0236] The difference between the preparation method of this embodiment and the film embodiment 1 is that the diamine in step (1) is replaced by a mixed diamine of a diamine monoboron compound 3 and 4,4'-diaminodiphenyl ether (ODA), the mixed molar ratio is 2:8, and PAA-9 is obtained by polymerization, and then polyimide PI-9 is obtained by curing at 350°C. The Young's modulus of the polyimide PI-9 is 3.00 Gpa, the dielectric constant is 2.99 at 10 GHz, the dielectric loss is 5.8‰ at 10 GHz, and the transmittance at 450 nm is 96%.
[0237] Film Example 15, conforming to Formula B-4:
[0238] The difference between the preparation method of this embodiment and the film embodiment 1 is that the diamine in step (1) is replaced by a diamine monoboron compound 4, and PAA-10 is obtained by polymerization, and then polyimide PI-10 is obtained by curing at 350° C. The Young's modulus of the polyimide PI-10 is 3.06 GPa, the dielectric constant is 3.04 at 10 GHz, the dielectric loss is 7.0‰ at 10 GHz, and the transmittance at 450 nm is 90%.
[0239] Film Example 16, conforming to Formula B-4:
[0240] The difference between the preparation method of this embodiment and the film embodiment 1 is that the diamine in step (1) is replaced by a mixed diamine of a diamine monoboron compound 4 and 4,4'-diaminodiphenyl ether (ODA), the mixed molar ratio is 1:9, and PAA-11 is obtained by polymerization, and then the polyimide PI-11 is obtained by curing at 350°C. The Young's modulus of the polyimide PI-11 is 3.23 GPa, the dielectric constant at 10 GHz is 3.11, the dielectric loss at 10 GHz is 9.2‰, and the transmittance at 450 nm is 87%.
[0241] Film Example 17, conforming to Formula B-4:
[0242] The difference between the preparation method of this embodiment and the film embodiment 1 is that the diamine in step (1) is replaced by a mixed diamine of a diamine monoboron compound 4 and 4,4'-diaminodiphenyl ether (ODA), the mixed molar ratio is 2:8, and PAA-12 is obtained by polymerization, and then the polyimide PI-12 is obtained by curing at 350°C. The polyimide PI-12 has a Young's modulus of 3.33 GPa, a dielectric constant of 3.02 at 10 GHz, a dielectric loss of 7.4‰ at 10 GHz, and a transmittance of 90% at 450 nm.
[0243] The above examples demonstrate that the polyimide polymer derived from the diamine monoboron compound of the present invention has excellent dielectric and optical properties. Figure 4 The dielectric properties of film examples 1, 9, 12, 15 and film comparative example 1 are compared. From the data in the figure, it can be clearly concluded that the polyimide film of the present invention has more excellent dielectric properties and meets the requirements for industrial application of flexible OLED display substrates. The diamine monoboron compound obtained by the present invention has broad application scenarios and application potential.
[0244] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A diamine monoboron compound, characterized in that: The diamine monoboron compound has a general structure as shown in at least one of the general formulas A-1 to A-4, wherein R1 and R2 are independently selected from hydrogen, deuterium, methyl, phenyl, methoxy, trifluoromethyl, tert-butyl, naphthyl, anthracenyl, silane, halogen, pyrazine, pyridine, pyrimidine, benzimidazole ring, carbazole, indolecarbazole, phenoxazine, phenothiazine, phenoselenazine, phenanthroimidazole, substituted or unsubstituted C2-C 10 Straight chain alkyl, substituted or unsubstituted C2~C 10 Branched alkyl, substituted or unsubstituted C7~C 30 Aryl, substituted or unsubstituted C2~C 10 Alkoxy, substituted or unsubstituted C1~C 10 Alkylamino, substituted or unsubstituted C2~C 10 Silane group.
2. The diamine monoboron compound according to claim 1, characterized in that: The R1 group is selected from hydrogen, methyl, phenyl, trifluoromethyl, tert-butyl, halogen, pyrazine, pyridine, pyrimidine, phenoxazine, phenothiazine, and phenoselenazine; the R2 group is selected from hydrogen, methyl, trifluoromethyl, tert-butyl, and halogen.
3. The diamine monoboron compound according to claim 1, characterized in that: The structural formula of the diamine monoboron compound is shown in any one of Formula 1 to Formula 144:
4. A polyimide polymer derived from a diamine monoboron compound as claimed in any one of claims 1 to 3, characterized in that: The polyimide polymer has a general structure as shown in at least one of the general formulas B-1 to B-4: Wherein, Ar is a tetravalent aromatic group; n is a natural number from 1 to 1000; The general formula B-1 is constructed from a diamine monoboron compound satisfying the general formula A-1; The general formula B-2 is constructed from a diamine monoboron compound satisfying the general formula A-2; The general formula B-3 is constructed by a diamine monoboron compound satisfying the general formula A-3; The general formula B-4 is constructed from a diamine monoboron compound satisfying the general formula A-4.
5. The polyimide polymer according to claim 4, characterized in that Ar is selected from:
6. Use of the diamine monoboron compound according to any one of claims 1 to 3 and / or the polyimide polymer according to any one of claims 4 to 5 in an organic electroluminescent device.
7. The use according to claim 6, characterized in that The diamine monoboron compound is specifically used as a guest luminescent material in the luminescent layer of an organic electroluminescent device; The polyimide polymer is specifically used as a thin film material in a flexible substrate of an organic electroluminescent device.
8. The use according to claim 6, characterized in that The organic electroluminescent device comprises in sequence: an anode, a hole injection layer, a hole transport layer, a light emitting layer, an electron transport layer, an electron injection layer, and a cathode; Preferably, an electron blocking layer or an exciton blocking layer is further provided between the hole transport layer and the light emitting layer; and a hole blocking layer or an exciton blocking layer is further provided between the light emitting layer and the electron transport layer.
Citation Information
Patent Citations
Polycyclic aromatic compound and composition for forming light emitting layer
CN107406759A
Condensed cyclic compound and organic light-emitting device including the same
CN111793079A
Organic electroluminescent device and fused polycyclic compound
CN112194672A
Mono-boron derivative based on fluorene and aniline fusion donor as well as preparation and application of mono-boron derivative
CN114891032A
Light emitting device and fused polycyclic compound for light emitting device
US20230130170A1