Phosphonated polymer, polyfunctional group compound and ion exchange membrane

The phosphonic polymer grafted through C-O-P structure is combined with the sulfonated polymer to form a double ion transport channel and ion cross-linking structure, which solves the problem of insufficient ion transport capability of phosphonic polymer under high temperature and low humidity conditions, and improves its Performance and stability in applications such as fuel cells.

CN119060222APending Publication Date: 2024-12-03FOSHAN LVDONG HYDROGEN ENERGY TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411212692.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing phosphonic polymer has poor ion transport capability under high temperature and low humidity conditions, and its solubility and processing performance are poor, which limits its use in fuel cells and other applications.

Method used

The phosphonic polymer grafted with C-O-P structure is used to form a multifunctional complex by complexing with the sulfonated polymer, forming a double-ion transport channel and ion cross-linking structure, thereby improving conductivity and mechanical properties.

Benefits of technology

It significantly improves the solubility, ion transport capability and stability of phosphonic polymers, enhances the tensile strength, chemical durability and electrochemical properties of the ion exchange membrane, and is suitable for applications under different temperature and humidity conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060222A_ABST
    Figure CN119060222A_ABST
Patent Text Reader

Abstract

The invention discloses a phosphonated polymer, a polyfunctional group compound and an ion exchange membrane, in a side chain structure of the phosphonated polymer, a phosphonic acid group is connected to a benzene ring through an alkoxy group or an oxy group, and compared with a phosphonated polymer with phosphonic acid grafted by a C-P bond, the phosphonated polymer has the advantages that the phosphonic acid group is more stable; the phosphonic acid polymer grafted with the C-O-P structure has better dissolving processability, ion transmission capacity and stability, preparation conditions are mild, side reactions of products are few, and the phosphonic acid polymer has a wider application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer materials, and in particular relates to a phosphonated polymer, a multifunctional group complex and an ion exchange membrane. Background Art

[0002] Fuel cell technology, water electrolysis hydrogen production technology and liquid flow battery technology are clean energy technologies that are crucial to the sustainable development of global energy. Ion exchange membranes made of sulfonated polymers are one of the key materials for these technologies. They have good conductivity under suitable temperature and high humidity conditions, but their ion transport performance is not ideal under high temperature and low humidity conditions.

[0003] The phosphonic acid functional group in the phosphonated polymer has the characteristics of proton acid and Lewis base, and is a typical zwitterionic group. On the one hand, the phosphonic acid functional group of the phosphonated polymer can ionize hydrogen ions in water, showing the characteristics of monobasic acid; on the other hand, the phosphonic acid functional group can combine with water molecules to form monovalent cations, and then can be complexed with acidic anions, showing the characteristics of Lewis base. Phosphonated polymers have higher water retention and lower proton transfer energy barriers under high temperature and low humidity conditions, but the current phosphonated polymers have poor ion transfer capacity, and the phosphonated polymers containing CP structure have poor solubility. The ion exchange membrane prepared from a single material has low conductivity, and it is easy to precipitate after mixing with other polymers, making it difficult to process and shape. Summary of the invention

[0004] The present invention is based on the inventor's discovery and understanding of the following facts and problems: It has been found through research that the multifunctional complex obtained by compounding a phosphonated polymer with a sulfonated polymer can form an ion crosslinking structure and a dual ion transmission channel, thereby obtaining a high-performance ion exchange membrane. Among them, phosphonated polyvinyl alcohol and phosphonated ethylene-vinyl alcohol copolymer contain a large number of hydroxyl groups, and the chemical stability and thermal stability of the multifunctional complex need to be further improved. The hydroxyl groups are easy to crosslink with the sulfonic acid functional groups to form sulfonates at high temperatures, which reduces the electrochemical and mechanical properties of the complex; polyvinylphosphonic acid has poor thermal stability and is easy to form a phosphonic anhydride crosslinking structure at high temperatures, which sharply reduces the electrochemical properties of the complex; phosphonated polystyrene and phosphonated polypentafluorostyrene have good thermal stability, are not easy to form phosphonic anhydride at high temperatures, and will not undergo covalent bond crosslinking with the sulfonic acid functional groups, but their poor processing performance limits their application.

[0005] The present invention aims to solve at least one of the technical problems in the related art to a certain extent. To this end, the embodiments of the present invention provide a phosphonated polymer, a multifunctional group complex and an ion exchange membrane. Compared with the phosphonated polymer grafted with phosphonic acid by CP bond, the phosphonated polymer grafted with COP structure has better solubility and processability, ion transmission capacity and stability, and the preparation conditions are relatively mild, the product has few side reactions and the anhydride structure is easy to hydrolyze, and has a broader application prospect.

[0006] An embodiment of the present invention provides a phosphonated polymer, wherein the phosphonated polymer comprises a repeating unit A0 represented by formula (1):

[0007]

[0008] Wherein, R2 is selected from H or F;

[0009] R3 is selected from H, F or CH3;

[0010] d is an integer selected from 0 to 12;

[0011] R4 is at least one selected from H, a C1-C6 alkyl group or an alkali metal.

[0012] Advantages and technical effects of the phosphonated polymers of the embodiments of the present invention: the phosphonated polymers have good chemical stability and solubility. Compared with the phosphonated polymers of CP bond-grafted phosphonic acid, the phosphonated polymers of the present invention of COP grafted phosphonic acid have better solubility and are conducive to solution molding processing. The hydrophilicity of the phosphonic acid group of the CP structure is poor, which is not conducive to the transmission of water and ions. The acid type of the phosphonic acid group of the COP structure and the phosphonic acid group of the CP structure are basically the same, but the longer side chain structure of the former is conducive to the movement of free water, which can improve the hydrophilicity and ion transmission capacity of the material. In addition, the oxygen atoms in COP can improve the flexibility of the phosphonated polymer material, making the material less likely to break due to a small amount of deformation during use. In addition, the main chain structure with high stability can improve the free radical resistance of the phosphonated polymer. The phosphonated polymer with a block structure not only improves the chemical stability of the phosphonated polymer, but also has a significant effect on the regulation of the phase structure in the ion exchange membrane when used for ion exchange membranes, and is more likely to form a larger phase separation structure to promote the transmission of ions. The phosphonated polymer grafted with a COP structure in the present invention has better solubility and processability, ion transport capacity and stability, relatively mild preparation conditions, few product side reactions, and anhydride structures are easily hydrolyzed, and has broader application prospects.

[0013] In some embodiments, the phosphonated polymer further comprises a repeating unit A1:

[0014]

[0015] Wherein, R2 is selected from H or F; R3 is selected from H, F or CH3; R6 is selected from H, Cl~C 12 Alkyl, C1-C6 perfluoroalkyl or C6-C 12 At least one of the aromatic groups;

[0016] And / or, the phosphonated polymer further comprises a repeating unit A2, wherein the repeating unit A2 comprises At least one of -CH2CH2-, -CH(CH3)CH2-, -CH(CH2CH3)CH2- or -C(CH3)2CH2-;

[0017] And / or, the phosphonated polymer further comprises a repeating unit A3:

[0018]

[0019] Wherein, R2 is selected from H or F; R3 is selected from H, F or CH3; d is selected from an integer of 0 to 12.

[0020] In some embodiments, the molar percentage of the repeating unit A0 in all the repeating units containing a benzene ring in the phosphonated polymer is defined as the phosphonation degree of the phosphonated polymer; the phosphonation degree is ≥ 0.1%;

[0021] and / or, the M of the phosphonated polymer n 30,000 to 1,200,000;

[0022] and / or, the M of the phosphonated polymer w 30,000 to 1,600,000;

[0023] And / or, the EW of the phosphonated polymer is 216 to 5000 g / mol.

[0024] The embodiment of the present invention provides a method for preparing a phosphonated polymer, comprising: subjecting a hydroxyl functionalized polymer to a phosphonating agent for phosphonation reaction to obtain the phosphonated polymer.

[0025] In the embodiment of the present invention, the synthesis conditions of the phosphonated polymer with COP structure are relatively simple and mild, and water and oxygen are allowed to exist during the phosphonation reaction, and there is no need to use high concentration of proton acid or anhydrous trimethylsilane for acidification. The side reaction of the reaction is the formation of phosphonic anhydride structure between different phosphonic acid groups. The degree of this side reaction is low, and it usually does not affect the dissolution and processing of the phosphonated polymer, and the phosphonic anhydride structure is easily hydrolyzed into phosphonic acid groups, which has little effect on the application scenarios with high humidity. Relatively speaking, the synthesis conditions of the phosphonated polymer grafted with CP structure are relatively harsh, and the acidification process is prone to the occurrence of cross-linking side reactions, which are basically irreversible, and the phosphonated polymer cannot become a fluid (melt or solution) for further processing and molding, which limits the application of the phosphonated polymer. The phosphonated polymer grafted with COP structure in the present invention has the advantages of good dissolution and processability, relatively mild preparation conditions, few product side reactions, and easy hydrolysis of anhydride structure.

[0026] In some embodiments, the hydroxyl-functional polymer is a hydroxyl-functional styrenic polymer;

[0027] And / or, the phosphonating agent includes at least one of orthophosphoric acid, oligophosphoric acid with a degree of polymerization less than 10 and its salt, sodium hexametaphosphate, phosphorus trichloride, phosphorus pentachloride, phosphorus oxychloride, and phosphite triester compounds;

[0028] and / or, the mass ratio of the hydroxyl functionalized polymer to the phosphonating agent is 1:0.2-10;

[0029] And / or, the temperature of the phosphonation reaction is 20-180°C;

[0030] And / or, the phosphonation reaction time is 1 min-24 h.

[0031] In some embodiments, the phosphonating agent includes orthophosphoric acid, and the hydroxyl-functionalized polymer is subjected to a phosphonating reaction with the phosphonating agent in the presence of a catalyst to obtain a phosphonated polymer.

[0032] In some embodiments, the catalyst comprises at least one of urea, urea derivatives, guanidine, guanidine derivatives, or C3-C6 amines;

[0033] And / or, the mass ratio of the hydroxyl functionalized polymer to the catalyst is 1:0.2-15.

[0034] The embodiment of the present invention provides a multifunctional complex, including a phosphonated polymer and a sulfonated polymer. The phosphonated polymer includes the phosphonated polymer described in the embodiment of the present invention or the phosphonated polymer prepared by the preparation method.

[0035] In the embodiment of the present invention, the dual ion transmission channel and ion cross-linking effect are formed between the phosphonic acid group and the sulfonic acid group in the multifunctional complex, which can improve the conductivity under all temperature and humidity conditions, regulate the water absorption rate and enhance the barrier property, dimensional stability and chemical stability. The phosphonated polymer in the multifunctional complex has good solubility, which is conducive to dispersion in the solution for blending and molding processing. When the multifunctional complex is applied to fuel cells, it has good comprehensive performance under different temperatures and humidities.

[0036] In some embodiments, the composition comprises 0.1% to 99.9% of the phosphonated polymer and 0.1% to 99.9% of the sulfonated polymer by mass;

[0037] And / or, the sulfonated polymer includes at least one of perfluorosulfonic acid resin, polyacid side chain perfluoro resin, sulfonated polytrifluorostyrene, sulfonated polysulfone, sulfonated polyethersulfone, sulfonated polyetheretherketone, sulfonated polyaryletherketone, sulfonated polyarylethernitrile, sulfonated polyphosphazene, sulfonated polyphenylene oxide, sulfonated polybenzonitrile, sulfonated polyimide or sulfonated polybenzimidazole.

[0038] The embodiment of the present invention provides a method for preparing a multifunctional complex, comprising: dispersing a phosphonated polymer and a sulfonated polymer in a solvent to obtain a dispersion; and drying the dispersion to obtain a multifunctional complex.

[0039] An embodiment of the present invention provides an ion exchange membrane, comprising the phosphonated polymer or the multi-functional complex described in the embodiment of the present invention.

[0040] In the embodiment of the present invention, the ion exchange membrane has all the advantages of the phosphonated polymer or the multifunctional complex, which will not be described in detail here. In addition, in the ion exchange membrane containing the multifunctional complex, the ion exchange membrane includes the phosphonated polymer and the sulfonated polymer, the ion pair effect of the phosphonic acid and the sulfonic acid, the hydrogen bonding effect between the various functional groups, the ionic cross-linking effect and the multi-ion transmission channel, which can enhance the tensile strength of the ion exchange membrane, improve the dimensional stability, chemical durability, barrier properties, electrochemical properties, mechanical properties, and service life, and have better comprehensive performance.

[0041] In some embodiments, the ion exchange membrane has a thickness of 3 to 500 μm;

[0042] and / or, the ion exchange capacity of the ion exchange membrane is 0.1 to 6.2 mmol / g;

[0043] And / or, the ion exchange membrane further comprises a porous reinforced membrane; the phosphonated polymer or multi-functional complex is supported on the porous reinforced membrane.

[0044] An embodiment of the present invention provides a method for preparing an ion exchange membrane, comprising: dispersing a phosphonated polymer in a solvent or dispersing a phosphonated polymer and a sulfonated polymer in a solvent or dispersing a multifunctional complex in a solvent to obtain a dispersion; forming a film from the dispersion and drying it to obtain an ion exchange membrane.

[0045] The embodiment of the present invention provides an application of a phosphonated polymer or a multifunctional complex or an ion exchange membrane, which is used for at least one of a battery, a water electrolysis hydrogen production device, a chlor-alkali industry, electrodialysis, osmosis, a sensor, and a supercapacitor. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 are cross-sectional SEM images of PEM-14 and D-PEM-14.

[0047] Figure 2 are TEM images of PEM-15 and D-PEM-14.

[0048] Figure 3 It is the polarization curve of PEM-14 at a temperature of 95°C and a humidity of 10-50% RH.

[0049] Figure 4 It is the polarization curve of D-PEM-14 at a temperature of 95°C and a humidity of 10-50% RH. DETAILED DESCRIPTION

[0050] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to be used to explain the present invention, but should not be understood as limiting the present invention.

[0051] A phosphonated polymer according to an embodiment of the present invention comprises a repeating unit A0 represented by formula (1):

[0052]

[0053] Wherein, R2 is selected from H or F;

[0054] R3 is selected from H, F or CH3;

[0055] d is an integer selected from 0 to 12, specifically, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, preferably an integer selected from 0 to 6, more preferably 0 or 1;

[0056] R4 is selected from at least one of H, C1-C6 alkyl or alkali metal; optionally, C1-C6 alkyl is selected from at least one of methyl, ethyl, propyl, butyl, pentyl and hexyl; optionally, alkali metal is selected from at least one of Li, Na and K; preferably, R4 is selected from at least one of H, methyl, ethyl, Li, Na and K; more preferably, R4 is selected from H;

[0057] Optionally, the positions of the two substituents on the benzene ring of the repeating unit A0 are selected from at least one of the ortho position, meta position or para position.

[0058] In the embodiment of the present invention, the phosphonated polymer has good chemical stability and solubility. Compared with the phosphonated polymer of phosphonic acid grafted with CP bond, the phosphonated polymer of COP grafted with phosphonic acid of the present invention has better solubility, which is conducive to solution molding processing. The hydrophilicity of the phosphonic acid group of the CP structure is poor, which is not conducive to the transmission of water and ions. The acid type of the phosphonic acid group of the COP structure and the phosphonic acid group of the CP structure are basically the same, but the longer side chain structure of the former is conducive to the movement of free water, which can improve the hydrophilicity and ion transmission capacity of the material. In addition, the oxygen atoms in COP can improve the flexibility of the phosphonated polymer material, so that the material is not easy to break due to a small amount of deformation during use. In addition, the main chain structure with high stability can improve the free radical resistance of the phosphonated polymer. The phosphonated polymer with a block structure not only improves the chemical stability of the phosphonated polymer, but also has a significant effect on the regulation of the phase structure in the ion exchange membrane when used for ion exchange membranes, and is more likely to form a larger phase separation structure, which promotes the transmission of ions. The phosphonated polymer grafted with a COP structure in the present invention has better solubility and processability, ion transport capacity and stability, relatively mild preparation conditions, few product side reactions, and anhydride structures are easily hydrolyzed, and has broader application prospects.

[0059] In some embodiments, the phosphonated polymer further comprises a repeating unit A1 represented by formula (2):

[0060]

[0061] In the formula, R2 is selected from H or F; R3 is selected from H, F or CH3;

[0062] R6 is selected from H, C1~C 12 Alkyl, C1-C6 perfluoroalkyl or C6-C 12 At least one of the aryl groups is preferably selected from H, C1-C4 alkyl or phenyl, more preferably selected from H or methyl;

[0063] Optionally, the positions of the two substituents on the benzene ring of the repeating unit A1 are selected from at least one of the ortho position, meta position or para position.

[0064] In some embodiments, the phosphonated polymer further comprises a repeating unit A2, wherein the repeating unit A2 comprises At least one of -CH2CH2-, -CH(CH3)CH2-, -CH(CH2CH3)CH2- or -C(CH3)2CH2-, preferably at least one of -CH2CH2-, -C(CH3)2CH2- or -CH(CH2CH3)CH2-.

[0065] In some embodiments, the phosphonated polymer further comprises a repeating unit A3 represented by formula (3):

[0066]

[0067] In the formula, R2 is selected from H or F; R3 is selected from H, F or CH3;

[0068] d is an integer selected from 0 to 12, specifically, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, preferably an integer selected from 0 to 6, more preferably 0 or 1;

[0069] Optionally, the positions of the two substituents on the benzene ring of the repeating unit A3 are selected from at least one of the ortho position, meta position or para position.

[0070] In some embodiments, the phosphonated polymer further comprises at least one of a repeating unit A1 represented by formula (2), a repeating unit A2, or a repeating unit A3 represented by formula (3).

[0071] In some embodiments, the phosphonated polymer is a polymer comprising (q1-q0-q3) repeating units A1, q0 repeating units A0 and q3 repeating units A3; or, the phosphonated polymer is a random copolymer or block copolymer comprising (q1-q0-q3) repeating units A1, q0 repeating units A0, q3 repeating units A3 and q2 repeating units A2;

[0072] Optionally, q0 is an integer from 200 to 8000, preferably an integer from 400 to 6000, and more preferably an integer from 500 to 4800;

[0073] q1 is an integer from 200 to 8000, preferably an integer from 400 to 7000, more preferably an integer from 500 to 6000;

[0074] q2 is an integer of 250 to 8000, preferably an integer of 400 to 6000, more preferably an integer of 500 to 4800;

[0075] q3 is an integer of 0-6000, preferably an integer of 0-1000, and more preferably an integer of 0-500.

[0076] In some embodiments, in the phosphonated polymer, the molar percentage of the repeating unit A0 in all the repeating units containing a benzene ring in the phosphonated polymer is defined as the phosphonation degree of the phosphonated polymer; in a specific embodiment, the molar amount of the repeating unit A0 in the phosphonated polymer is N0, the sum of the molar amounts of the repeating unit A0, the repeating unit A1 and the repeating unit A3 is N1, and the ratio of N0 to N1 is defined as the phosphonation degree of the phosphonated polymer;

[0077] Optionally, the phosphonation degree of the phosphonated polymer is ≥0.1%, specifically, for example, 0.1%, 0.5%, 1%, 2%, 5%, 10%, 20%, 50%, preferably, the phosphonation degree is ≥0.5%, more preferably, the phosphonation degree is ≥2%.

[0078] In some embodiments, the M of the phosphonated polymer is n The M of the phosphonated polymer is 30,000 to 1,200,000, preferably 40,000 to 800,000, more preferably 50,000 to 600,000. w It is 30,000-1,600,000, preferably, 40,000-1,000,000, more preferably, 50,000-800,000.

[0079] In some embodiments, the EW of the phosphonated polymer is 216 to 5000 g / mol, preferably, 217 to 3000 g / mol, more preferably, 220 to 2000 g / mol.

[0080] In some embodiments, the phosphonated polymer comprises at least one of the chemical structures of formula (4) to formula (13) in Table 1.

[0081] Table 1

[0082]

[0083]

[0084] A method for preparing a phosphonated polymer according to an embodiment of the present invention comprises: subjecting a hydroxyl functionalized polymer to a phosphonating agent for phosphonation reaction to obtain the phosphonated polymer.

[0085] In the embodiment of the present invention, the synthesis conditions of the phosphonated polymer with COP structure are relatively simple and mild, and water and oxygen are allowed to exist during the phosphonation reaction, and there is no need to use high concentration of proton acid or anhydrous trimethylsilane for acidification. The side reaction of the reaction is the formation of phosphonic anhydride structure between different phosphonic acid groups. The degree of this side reaction is low, and it usually does not affect the dissolution and processing of the phosphonated polymer, and the phosphonic anhydride structure is easily hydrolyzed into phosphonic acid groups, which has little effect on the application scenarios with high humidity. Relatively speaking, the synthesis conditions of the phosphonated polymer grafted with CP structure are relatively harsh, and the acidification process is prone to the occurrence of cross-linking side reactions, which are basically irreversible, and the phosphonated polymer cannot become a fluid (melt or solution) for further processing and molding, which limits the application of the phosphonated polymer. The phosphonated polymer grafted with COP structure in the present invention has the advantages of good dissolution and processability, relatively mild preparation conditions, few product side reactions, and easy hydrolysis of anhydride structure.

[0086] In some embodiments, the hydroxyl-functionalized polymer is a hydroxyl-functionalized styrenic polymer; alternatively, the hydroxyl-functionalized polymer comprises a phenolic hydroxylated styrenic polymer or a hydroxymethylated styrenic polymer.

[0087] In some embodiments, the hydroxyl-functional polymer is dispersed in an organic medium and then subjected to a phosphonation reaction with a phosphonating agent to obtain a phosphonated polymer.

[0088] In some embodiments, the structural formula of the hydroxyl-functionalized polymer is selected from at least one of the structural formulas shown in formula (14) or formula (15):

[0089]

[0090] In some embodiments, the hydroxyl-functionalized polymer is a polymer comprising (q1-q3) repeating units A1 and q3 repeating units A3; or, the hydroxyl-functionalized polymer is a random copolymer or block copolymer comprising (q1-q3) repeating units A1, q3 repeating units A3 and q2 repeating units A2;

[0091] Optionally, q1 is an integer from 200 to 8000, preferably an integer from 400 to 7000, more preferably an integer from 500 to 6000;

[0092] q2 is an integer of 250 to 8000, preferably an integer of 400 to 6000, more preferably an integer of 500 to 4800;

[0093] q3 is an integer of 0-6000, preferably an integer of 0-1000, and more preferably an integer of 0-500.

[0094] In some embodiments, in the hydroxy-functionalized polymer, the molar amount of repeating unit A3 is N3, the sum of the molar amounts of repeating unit A1 and repeating unit A3 is N1, and the ratio of N3 to N1 is defined as the degree of functionalization of the hydroxy-functionalized polymer;

[0095] Optionally, the functionalization degree of the hydroxyl functionalized polymer is ≥5%, specifically, for example, 5%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, 99%, 100%, preferably, ≥20%, further preferably, ≥50%, more preferably, ≥80%. In the embodiment of the present invention, when the functionalization degree is too low, the fewer sites available for grafting phosphonic acid functional groups, the weaker the ion exchange capacity of the subsequently prepared phosphonated polymer.

[0096] In some embodiments, the hydroxyl-functionalized polymer is obtained by polymerization of monomers, or by hydroxyl-functionalization reaction of a styrene polymer; optionally, the preparation method of the hydroxyl-functionalized polymer comprises a substitution reaction of an alkoxy styrene polymer or a halomethylated styrene polymer, optionally, the alkoxy styrene polymer is subjected to a substitution reaction by acidification treatment to obtain a phenolic hydroxylated styrene polymer.

[0097] In some embodiments, the styrene polymer is a polymer comprising q1 repeating units A1, or the styrene polymer is a random copolymer or a block copolymer comprising q1 repeating units A1 and q2 repeating units A2;

[0098] Optionally, q1 is an integer from 200 to 8000, preferably an integer from 400 to 7000, more preferably an integer from 500 to 6000;

[0099] q2 is an integer of 250 to 8000, preferably, an integer of 400 to 6000, more preferably, an integer of 500 to 4800.

[0100] In a specific embodiment, the styrene polymer includes polystyrene, poly(3-methylstyrene), poly(4-methylstyrene), poly(α-methylstyrene), poly(styrene-ran-α-methylstyrene), polytrifluorostyrene, poly(styrene-ran-ethylene), poly(styrene-ran-butylene), poly(styrene-b-ethylene), poly(styrene-b-(ethylene-ran-butylene)-b-styrene) (SEBS), poly(styrene-b-(ethylene-ran-propylene)-b-styrene) (SEPS), poly(styrene-b-(ethylene-ethylene)-b-styrene) (SEPS), poly(styrene-b-(ethylene-propylene ... -propylene)-b-styrene) (SEEPS), poly(styrene-b-isobutylene-b-styrene) (SIBS); preferably, it includes at least one of polystyrene, poly(3-methylstyrene), poly(4-methylstyrene), poly(α-methylstyrene), poly(styrene-ran-α-methylstyrene), polytrifluorostyrene, SEBS, SEPS, SEEPS, SIBS; more preferably, it includes at least one of polystyrene, poly(4-methylstyrene), poly(α-methylstyrene), polytrifluorostyrene, SEBS, SIBS.

[0101] In some embodiments, the phosphonating agent includes at least one of orthophosphoric acid, oligophosphoric acid with a degree of polymerization less than 10 and its salt, sodium hexametaphosphate, phosphorus trichloride, phosphorus pentachloride, phosphorus oxychloride, and phosphite triester compounds;

[0102] Optionally, the oligomeric phosphoric acid with a degree of polymerization less than 10 and its salt include oligomeric phosphoric acid with a degree of polymerization less than 10, alkali metal salt or ammonium salt of oligomeric phosphoric acid with a degree of polymerization less than 10; the alkali metal includes at least one of lithium, sodium and potassium; the triester phosphite compound includes at least one of trimethyl phosphite and triethyl phosphite;

[0103] Preferably, the phosphonating agent comprises at least one of orthophosphoric acid, trimethyl phosphite and triethyl phosphite; more preferably, orthophosphoric acid.

[0104] In the embodiment of the present invention, the phosphonation reaction of oligophosphoric acid and its salts, phosphorus (oxy) chloride and the like as the phosphonation reagent does not require a catalyst.

[0105] In some embodiments, the mass ratio of the hydroxyl-functionalized polymer to the phosphonating agent is 1:0.2-10, specifically, 1:0.2-10 (eg, 0.2, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10).

[0106] In some embodiments, the phosphonating agent includes orthophosphoric acid, and the hydroxyl-functionalized polymer is subjected to a phosphonating reaction with the phosphonating agent to obtain a phosphonated polymer;

[0107] Optionally, the hydroxyl functionalized polymer and the phosphonating agent are subjected to a phosphonating reaction under the action of a catalyst to obtain a phosphonated polymer;

[0108] Optionally, the catalyst comprises at least one of urea, urea derivatives, guanidine, guanidine derivatives or C3-C6 amines, and optionally, the C3-C6 amine comprises at least one of trimethylamine and triethylamine; optionally, the guanidine derivative comprises dicyandiamide; preferably, the catalyst comprises urea and dicyandiamide; further preferably, the mass ratio of urea to dicyandiamide is 0-6:0-9, specifically, 0-6 (e.g., 0, 0.2, 0.3, 0.5, 1, 2, 3, 5, 6): 0-9 (e.g., 0, 0.2, 0.3, 0.5, 1, 2, 3, 5, 9);

[0109] The phosphonated polymer can be obtained without adding a catalyst.

[0110] In the embodiment of the present invention, the phosphonating agent orthophosphoric acid has the advantages of low viscosity, low cost, wide source and stable chemical properties, and the reaction system has no requirements on water content and gas atmosphere, and the reaction conditions are mild. Urea and dicyandiamide have wide sources, low cost and high catalytic efficiency. The reaction system composed of orthophosphoric acid, urea and dicyandiamide has the advantages of safety, high efficiency and low cost, and is the most preferred reaction system.

[0111] In some embodiments, the mass ratio of the hydroxyl-functional polymer to the catalyst is 1:0.2-15, specifically, 1:0.2-15 (e.g., 0.2, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 12, 15).

[0112] In some embodiments, the hydroxyl functionalized polymer is subjected to a phosphonation reaction with orthophosphoric acid in the presence of urea and dicyandiamide to obtain a phosphonated polymer;

[0113] Optionally, the mass ratio of the hydroxyl-functionalized polymer, orthophosphoric acid, urea and dicyandiamide is 1:0.2-10:0-6:0-9, specifically, 1:0.2-10 (for example, 0.2, 0.3, 0.5, 1, 2, 5, 8, 10):0-6 (for example, 0, 0.2, 0.3, 0.5, 1, 2, 3, 5, 6):0-9 (for example, 0, 0.2, 0.3, 0.5, 1, 2, 3, 5, 9); preferably, 1:0.3-5:0.2-5:0.2-5; more preferably, 1:0.5-3:0.2-3:0.3-3.

[0114] In the embodiment of the present invention, the mass ratio of the hydroxyl functional polymer, orthophosphoric acid, urea and dicyandiamide is conducive to the efficient reaction. If the orthophosphoric acid content is too little, the product phosphonation degree is relatively limited, and if the orthophosphoric acid content is too high, unnecessary waste will be caused and dispersion will be difficult. Not adding a catalyst or a small amount of catalyst will result in a relatively low reaction rate and a low degree of reaction. Too much catalyst will cause unnecessary waste and produce nitrogen-containing by-products.

[0115] In some embodiments, the organic medium includes at least one of a halogenated hydrocarbon, an aromatic hydrocarbon, an alkane, tetrahydrofuran, N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), tetramethyl sulfoxide, or dimethyl sulfoxide (DMSO);

[0116] Optionally, the organic medium includes at least one of chloroform, 1,2-dichloroethane, 1,1,2,2-tetrachloroethane, cyclohexane, toluene, xylene, o-dichlorobenzene, DMF, DMAC, DMSO or tetrahydrofuran; preferably, it includes at least one of cyclohexane, toluene, xylene, o-dichlorobenzene, DMF, DMAC or DMSO.

[0117] In some embodiments, the temperature of the phosphonation reaction is 20-180°C, specifically, for example, 20°C, 40°C, 60°C, 80°C, 100°C, 120°C, 140°C, 160°C, 180°C, preferably, 80-160°C;

[0118] And / or, the phosphonation reaction time is 1 min-24 h, specifically, for example, 1 min, 3 min, 7 min, 21 min, 0.5 h, 2 h, 10 h, 20 h, 24 h, preferably, 3 min-2 h.

[0119] In the embodiments of the present invention, under the appropriate feed ratio, reaction temperature and reaction time, hydroxyl-functionalized polymers of different main chain structures and side group structures (phenolic hydroxyl and alcoholic hydroxyl) can fully react with the phosphonating agent to obtain the phosphonated polymer. Low temperature, short reaction time or too little phosphonating agent will cause the hydroxyl groups of the polymer raw materials to react incompletely. The degree of phosphonation can be regulated by the reaction conditions, and can also be regulated by the grafting rate of the hydroxyl groups in the hydroxyl-functionalized polymer. By reasonably selecting the reaction raw materials and reaction conditions, a phosphonated polymer with a clear structure can be controllably prepared.

[0120] In some embodiments, the mass of the hydroxyl-functionalized polymer and the phosphonating agent is 0.1% to 40% of the mass of the organic medium, preferably 0.5% to 30%, more preferably 1% to 20% by mass;

[0121] Optionally, when a catalyst is used, the mass of the hydroxyl-functionalized polymer, the phosphonating agent and the catalyst is 0.1% to 40% of the mass of the organic medium, preferably 0.5% to 30%, more preferably 1% to 20%. In the embodiment of the present invention, the organic medium can effectively disperse the hydroxyl-functionalized polymer, the phosphonating agent and the catalyst.

[0122] In some embodiments, the hydroxyl-functionalized polymer is first dispersed in an organic medium to obtain a hydroxyl-functionalized polymer dispersion, and then a phosphonating agent or a phosphonating agent and a catalyst are added to perform a phosphonating reaction;

[0123] Optionally, the concentration of the hydroxyl-functional polymer dispersion is 1 mg / mL to 300 mg / mL, preferably, 5 mg / mL to 250 mg / mL, more preferably, 5 mg / mL to 200 mg / mL.

[0124] In some embodiments, after the phosphonation reaction is completed, the product is cooled to room temperature, then added to a poor solvent for precipitation, washed, and dried to obtain a phosphonated polymer solid product; optionally, the poor solvent includes at least one of water, acetone, butanone, fatty alcohol, and esters.

[0125] A multifunctional complex according to an embodiment of the present invention comprises a phosphonated polymer and a sulfonated polymer, wherein the phosphonated polymer is the phosphonated polymer according to an embodiment of the present invention or the phosphonated polymer prepared by the preparation method.

[0126] In the embodiment of the present invention, the dual ion transmission channel and ion cross-linking effect are formed between the phosphonic acid group and the sulfonic acid group in the multifunctional complex, which can improve the conductivity under all temperature and humidity conditions, regulate the water absorption rate and enhance the barrier property, dimensional stability and chemical stability. The phosphonated polymer in the multifunctional complex has good solubility, which is conducive to dispersion in the solution for blending and molding processing. When the multifunctional complex is applied to fuel cells, it has good comprehensive performance under different temperatures and humidities.

[0127] In some embodiments, the phosphonated polymer and the sulfonated polymer in the multifunctional complex are mixed in any ratio.

[0128] In some embodiments, the multifunctional complex comprises, by mass, 0.1% to 99.9% of the phosphonated polymer and 0.1% to 99.9% of the sulfonated polymer. Specifically, for example, the content of the phosphonated polymer is 0.1%, 1%, 5%, 10%, 20%, 30%, 50%, 80%, 90%, 99%, 99.9%, and the content of the sulfonated polymer is 0.1%, 1%, 5%, 10%, 20%, 30%, 50%, 80%, 90%, 99%, 99.9%. Preferably, it comprises 1% to 99% of the phosphonated polymer and 1% to 99% of the sulfonated polymer.

[0129] In some embodiments, the sulfonated polymer includes at least one of perfluorosulfonic acid resin, polyacid side chain perfluoro resin, sulfonated polytrifluorostyrene, sulfonated polysulfone, sulfonated polyethersulfone, sulfonated polyetheretherketone, sulfonated polyaryletherketone, sulfonated polyarylethernitrile, sulfonated polyphosphazene, sulfonated polyphenylene oxide, sulfonated polybenzonitrile, sulfonated polyimide or sulfonated polybenzimidazole;

[0130] Preferably, it comprises at least one of perfluorosulfonic acid resin, polyacid side chain perfluoro resin, sulfonated polytrifluorostyrene, sulfonated polyetheretherketone, sulfonated polyaryletherketone, and sulfonated polyarylethernitrile;

[0131] More preferably, it includes at least one of perfluorosulfonic acid resin, polyacid side chain perfluoro resin, and sulfonated polytrifluorostyrene.

[0132] In some embodiments, the sulfonated polymer or phosphonated polymer may bind different cations, including at least one of hydrogen ions, monovalent metal cations, ammonium ions, alkaline earth metal ions, or other multivalent cations;

[0133] Optionally, the cation includes at least one of hydrogen ion, ammonium ion, lithium ion, sodium ion, potassium ion, silver ion, magnesium ion, calcium ion, copper ion, iron ion, zirconium ion, cerium ion, manganese ion, aluminum ion, titanium ion, vanadium ion or zinc ion.

[0134] In some embodiments, the general structural formula of the perfluorosulfonic acid resin is:

[0135]

[0136] The general structural formula of the polyacid side chain type perfluororesin is:

[0137]

[0138] The general structural formula of the sulfonated polytrifluorostyrene is:

[0139]

[0140] Wherein, a=0-6, b=2-5, c=1-5, R1 is selected from H, F or CF3, and M is selected from the cations bound to the above-mentioned sulfonated polymers.

[0141] A method for preparing a multifunctional complex according to an embodiment of the present invention comprises: dispersing a phosphonated polymer and a sulfonated polymer in a solvent to obtain a dispersion; and drying the dispersion to obtain a multifunctional complex.

[0142] In the embodiment of the present invention, the multifunctional complex is prepared by a blending method, wherein the phosphonated polymer and the sulfonated polymer are dispersed in a solvent and dried to obtain the multifunctional complex. The preparation method of the multifunctional complex is simple to operate, easy to implement, and convenient for industrial promotion.

[0143] In some embodiments, the dispersion temperature is 10 to 240° C.; the dispersion pressure is normal pressure to 20 MPa; and the dispersion time is 0.1 to 24 h.

[0144] In some embodiments, the drying temperature is 20-180°C.

[0145] In some embodiments, the solvent includes at least one of water, a highly polar organic solvent, tetrahydrofuran, toluene, xylene, and a fatty alcohol; optionally, the highly polar organic solvent includes at least one of DMF, DMAC, DMSO, and hexamethylphosphoric acid triamide; optionally, the fatty alcohol includes at least one of methanol, ethanol, isopropanol, n-propanol, tert-butanol, n-butanol, n-hexanol, ethylene glycol, propylene glycol, and glycerol.

[0146] An ion exchange membrane according to an embodiment of the present invention comprises the phosphonated polymer or multi-functional complex according to an embodiment of the present invention.

[0147] In the embodiment of the present invention, the ion exchange membrane has all the advantages of the phosphonated polymer or the multifunctional complex, which will not be described in detail here. In addition, in the ion exchange membrane containing the multifunctional complex, the ion exchange membrane includes the phosphonated polymer and the sulfonated polymer, the ion pair effect of the phosphonic acid and the sulfonic acid, the hydrogen bonding effect between the various functional groups, the ionic cross-linking effect and the multi-ion transmission channel, which can enhance the tensile strength of the ion exchange membrane, improve the dimensional stability, chemical durability, barrier properties, electrochemical properties, mechanical properties, and service life, and have better comprehensive performance.

[0148] In some embodiments, the ion exchange membrane has a thickness of 3 to 500 μm, specifically, for example, 3 μm, 4 μm, 5 μm, 10 μm, 100 μm, 200 μm, 250 μm, 320 μm, 500 μm, preferably 4 to 320 μm, and more preferably 5 to 200 μm.

[0149] In some embodiments, the ion exchange capacity of the ion exchange membrane is 0.1 to 6.2 mmol / g, specifically, for example, 0.1 mmol / g, 0.15 mmol / g, 0.2 mmol / g, 1 mmol / g, 2.5 mmol / g, 3 mmol / g, 4 mmol / g, 6.2 mmol / g, preferably 0.15 to 4.0 mmol / g, and more preferably 0.2 to 2.5 mmol / g.

[0150] In some embodiments, the ion exchange membrane further comprises a porous reinforced membrane; the phosphonated polymer or multifunctional complex is loaded on the porous reinforced membrane, and optionally, the phosphonated polymer or multifunctional complex is loaded on one side or both sides of the porous reinforced membrane along the thickness direction thereof. In an embodiment of the present invention, the porous reinforced membrane is a reinforced layer of an ion exchange resin material, which is dispersed in the ion exchange resin of the ion exchange membrane.

[0151] In some embodiments, the porous reinforced membrane comprises at least one of a porous polyolefin membrane or a porous aromatic polymer membrane;

[0152] Optionally, the porous polyolefin membrane includes at least one of a porous polytetrafluoroethylene membrane, a polyvinylidene fluoride membrane, a polyhexafluoropropylene membrane, an ethylene-tetrafluoroethylene copolymer membrane, a polyethylene membrane, and a polypropylene membrane;

[0153] Optionally, the porous aromatic polymer membrane includes at least one of a porous polyarylether polymer membrane, a polyimide membrane, a polyphosphazene membrane, and a polybenzimidazole membrane; the porous polyarylether polymer membrane includes at least one of a porous polyarylethersulfone membrane, a polysulfone membrane, a polyethersulfone membrane, a polyaryletherketone membrane, and a polyaryletherketone derivative membrane.

[0154] In some embodiments, the mass percentage of the porous reinforced membrane in the ion exchange membrane is 0.1% to 90%, preferably 1% to 70%, and more preferably 3% to 50%.

[0155] A method for preparing an ion exchange membrane according to an embodiment of the present invention comprises: dispersing a phosphonated polymer in a solvent or dispersing a phosphonated polymer and a sulfonated polymer in a solvent or dispersing a multifunctional complex in a solvent to obtain a dispersion; forming a film from the dispersion and drying it to obtain an ion exchange membrane.

[0156] In some embodiments, the dispersion temperature is 10 to 240° C.; the dispersion pressure is normal pressure to 20 MPa; and the dispersion time is 0.1 to 24 h.

[0157] In some embodiments, after being dispersed in the solvent, mixing is performed by at least one of stirring, shaking, and ultrasound.

[0158] In some embodiments, the film forming method includes at least one of casting, coating or pouring; optionally, the coating includes at least one of slit coating or blade coating.

[0159] In some embodiments, the drying temperature is 20°C to 180°C.

[0160] In some embodiments, the ion exchange membrane further comprises a porous reinforced membrane, and the dispersion is coated on one side or both sides of the porous reinforced membrane and dried to obtain the ion exchange membrane.

[0161] In some embodiments, the solvent includes at least one of water, a highly polar organic solvent, tetrahydrofuran, toluene, xylene, and a fatty alcohol; optionally, the highly polar organic solvent is selected from at least one of DMF, DMAC, DMSO, and hexamethylphosphoric acid triamide; optionally, the fatty alcohol includes at least one of methanol, ethanol, isopropanol, n-propanol, tert-butanol, n-butanol, n-hexanol, ethylene glycol, propylene glycol, and glycerol.

[0162] In some embodiments, when the porous reinforced membrane comprises a porous polytetrafluoroethylene membrane, optionally, the content of DMSO, NMP and water in the solvent does not exceed 80%. In the embodiments of the present invention, since the porous polytetrafluoroethylene has low surface polarity and good solvent resistance, a certain amount of low polarity solvent is required to ensure that the dispersion has good wettability on the reinforced membrane, so as to better play the role of the reinforcement layer or facilitate coating.

[0163] In some embodiments, when the porous reinforced membrane includes a porous reinforced membrane other than a porous polytetrafluoroethylene membrane, optionally, the water content in the solvent does not exceed 80%. In the embodiments of the present invention, because other porous reinforced membranes generally have poor hydrophilicity, a certain amount of organic solvent is required to improve the wettability of the dispersion on the reinforced membrane, so as to better play the role of the reinforcement layer or facilitate coating.

[0164] The application of a phosphonated polymer or a multifunctional complex or an ion exchange membrane according to an embodiment of the present invention is used in at least one of a battery, a water electrolysis hydrogen production device, a chlor-alkali industry, electrodialysis, osmosis, a sensor, and a supercapacitor.

[0165] In some embodiments, the battery includes at least one of a primary battery and a secondary battery.

[0166] In some embodiments, the primary battery comprises an acid primary battery.

[0167] In some embodiments, the secondary battery includes at least one of a lithium battery, a flow battery, and a fuel cell.

[0168] In some embodiments, at least one of a proton exchange membrane for producing hydrogen by water electrolysis, an acidic primary battery membrane, a secondary battery membrane, a polyelectrolyte in a supercapacitor, and a polyelectrolyte membrane; optionally, the secondary battery membrane is a lithium battery membrane.

[0169] A fuel cell according to an embodiment of the present invention comprises the phosphonated polymer or multifunctional complex or ion exchange membrane according to an embodiment of the present invention.

[0170] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.

[0171] The test methods for conductivity, EW, IEC, tensile strength and water absorption refer to GB / T20042.3-2022 "Proton Exchange Membrane Fuel Cell Part 3: Proton Exchange Membrane Test Method". The test temperature for conductivity is 80°C and the relative humidity is 50% or 95%; or the test temperature for conductivity is 30°C and the test sample is immersed in water.

[0172] Fuel cell polarization curve: The test method refers to GB / T20042.5-2022 "Proton exchange membrane fuel cell Part 5: Membrane electrode test method".

[0173] Hydrogen permeation current: The test method refers to GB / T20042.5-2022 "Proton Exchange Membrane Fuel Cell Part 5: Membrane Electrode Test Method", and the test conditions are 80°C and 90% relative humidity. The hydrogen permeation current represents the permeation of hydrogen. The lower the hydrogen permeation current, the better the barrier property of the ion exchange membrane.

[0174] Free radical resistance: Soak the polymer material or ion exchange membrane in Fenton's reagent at 80°C for 8 hours, and compare the mass changes before and after soaking. The composition of Fenton's reagent: 50mL of 3% H2O2 solution, to which 0.1mL 0.01mol / L Fe 2+ The solution is the Fenton reagent. The Fenton reagent is prepared and used immediately. The greater the ratio of the remaining mass to the initial mass before immersion, the better the free radical resistance, which is expressed as the percentage of the remaining mass to the initial mass.

[0175] Liquid flow battery performance: The test method refers to NB / T42081-2016 "All-vanadium liquid flow battery single cell performance test method".

[0176] Ion permeability: The test method refers to NB / T42080-2016 "Test method for ion conduction membrane for all-vanadium redox flow battery". 1.5mol / L VOSO4 and 3mol / L sulfuric acid aqueous solution are used to simulate the electrolyte of all-vanadium redox flow battery to measure VO 2+The ion diffusion coefficient when it diffuses through the ion conductive membrane to the blank side of the deionized water, VO 2+ The change of concentration with time was measured by UV-Vis spectrophotometer. The smaller the ion permeability value, the better the ion barrier property of the membrane.

[0177] Gas barrier property: The gas barrier property of the ion exchange membrane is characterized by the oxygen permeability, and the test and calculation methods are carried out according to the national standard GB1038-2000. The smaller the oxygen permeability value, the better the gas barrier property of the ion exchange membrane.

[0178] The organic solvents, film-forming solvents, and phosphonating agents used in the examples are all common chemical reagents; poly(4-bromostyrene), polystyrene-co-α-methylstyrene, and poly(α-methylstyrene) are from MacLean or Aladdin; polytrifluorostyrene is from San Ai Fu; SEBS is from Kraton and Asahi Chemical; SIBS is from Zhongyuan Chemical; poly(4-methoxystyrene) is from ACROS; and styrene-b-(4-tert-butoxystyrene) diblock copolymer is from Polymer Source. The orthophosphoric acid in the examples is an orthophosphoric acid solution with a mass percentage concentration of 85%.

[0179] Example 1: Preparation of phenol hydroxylated styrene polymer

[0180] Weigh 2 g of poly (4-methoxystyrene) and dissolve it in 80 mL of DMAC, add 8 mL of concentrated hydrochloric acid (12 mol / L), heat and reflux for 12 h to convert the methoxy groups into phenolic hydroxyl groups, use methanol for precipitation, wash and dry to obtain poly (p-hydroxystyrene) (PSOH-1).

[0181] Example 2: Preparation of phenol hydroxylated styrene polymer

[0182] Different from Example 1, the raw material for the reaction is styrene-b-(4-tert-butoxystyrene) diblock copolymer, and styrene-b-(4-hydroxystyrene) diblock copolymer (PSOH-2) is obtained. The chemical structure of PSOH-2 is as follows:

[0183]

[0184] Example 3: Preparation of Chloromethylated Styrene Polymers

[0185] A certain amount of styrene polymer (containing about 50 mmol of repeating unit A1) was weighed and dispersed in chloroform, and 200 mmol of 1,4-dichloromethoxybutane was used as a chloromethylation reagent and 100 mmol of anhydrous tin tetrachloride was used as a catalyst to prepare a chloromethylated styrene polymer. The molar ratio of chloromethyl to benzene ring is defined as the chloromethylation degree, and the chloromethylation degree of all chloromethylated styrene polymers is 100%. The numbers of the chloromethylated styrene polymers and the styrene polymers are shown in Table 2.

[0186] Table 2

[0187] Chloromethylated styrene polymers Styrene polymers X-PS-3 <![CDATA[Poly(α-methylstyrene) (M w ~300000)]]> X-PS-4 Polytrifluorostyrene X-PS-5 SEBS (Asahi Kasei H1043, styrene content 67%) X-PS-6 Polystyrene-co-α-methylstyrene X-PS-7 SIBS (styrene content 30.3%)

[0188] Example 4: Preparation of bromomethylated styrene polymer

[0189] Weigh 7.08 g of poly (4-methylstyrene) (Sigma-Aldrich, M w ~72000), dispersed in dichloromethane, using 80mmol of N-bromosuccinimide as a bromination agent, to obtain a bromomethylated styrene polymer X-PS-8. The molar ratio of bromomethyl to benzene ring is defined as the bromomethylation degree, and the bromomethylation degree of X-PS-8 is 20.0%.

[0190] Example 5: Preparation of hydroxymethylated styrene polymers

[0191] 3 g of the halomethylated styrene polymer and PVBC in Example 3 and Example 4 were weighed respectively, dissolved and dispersed in 80 mL of toluene, 5 g of sodium acetate and 10 mL of an aqueous solution of 0.5 g of tetrabutylammonium bromide were added, stirred and reacted at 100° C. for 96 h, and poured into methanol for precipitation to obtain an esterified polymer solid. 1.5 g of the esterified polymer solid was dissolved in 100 mL of toluene, 4 g of KOH and 5 mL of an aqueous solution of 0.8 g of tetrabutylammonium bromide were added, stirred and reacted at 40° C. for 96 h, the product was precipitated in methanol, and vacuum dried to obtain a hydroxymethylated styrene polymer.

[0192] The halomethylated styrene polymer raw materials and the corresponding hydroxymethylated styrene polymer products are shown in Table 3. In Table 3, PVBC is poly (vinyl benzyl chloride) (from Sigma-Aldrich, referred to as "PVBC", M n ~55000,M w ~100000, a 60 / 40 mixture of 3-isomer and 4-isomer). The halomethyl groups of the halomethylated styrene polymer can be completely converted into hydroxymethyl groups, and the hydroxyl groups in the hydroxymethylated styrene polymer can be further reacted with a phosphonating agent to obtain a phosphonated polymer.

[0193] Table 3

[0194] Halomethylated polymers Hydroxymethylated styrene polymers X-PS-3 PSOH-3 X-PS-4 PSOH-4 X-PS-5 PSOH-5 X-PS-6 PSOH-6 X-PS-7 PSOH-7 X-PS-8 PSOH-8 PVBC PSOH-9

[0195] Example 6: Preparation of phosphonated polymer

[0196] Disperse 2g of hydroxyl functionalized polymer in an organic medium, add a certain amount of urea and dicyandiamide, stir to dissolve, then heat to reaction temperature, add a certain amount of orthophosphoric acid, stir to react for a certain period of time, then cool to room temperature, pour into a poor solvent for precipitation and washing, and dry to obtain a phosphonated polymer.

[0197] The reaction conditions for preparing the phosphonated polymer are shown in Tables 4 and 5, and the EW and degree of phosphonation of the phosphonated polymer are shown in Table 5.

[0198] Table 4

[0199]

[0200]

[0201] Table 5

[0202]

[0203] Under the appropriate feed ratio, reaction temperature and reaction time, hydroxyl-functionalized polymers with different main chain structures and side group structures (phenolic hydroxyl and alcoholic hydroxyl) can fully react with the phosphonating agent to obtain phosphonated polymers. Low temperature, short reaction time or insufficient phosphonating agent will cause incomplete reaction of the hydroxyl groups of the polymer raw materials. The degree of phosphonation can be regulated by the reaction conditions or by the grafting rate of the hydroxyl groups in the hydroxyl-functionalized polymer. By rationally selecting the reaction raw materials and reaction conditions, phosphonated polymers with clear structures can be prepared in a controllable manner.

[0204] Example 7 Preparation of ion exchange membrane

[0205] 0.25 g of the phosphonated polymer in Example 6 was weighed and dissolved in 5 mL of solvent to form a solution, which was then cast into an ultra-flat petri dish and dried at 80° C. for 6 h to obtain an ion exchange membrane with an average thickness of 50 μm. The phosphonated polymer, solvent composition and ion exchange capacity (IEC) of the ion exchange membrane are shown in Table 6. The ratio of the mixed solvent in Table 6 is the mass ratio.

[0206] Table 6

[0207]

[0208]

[0209] The phosphonate polymer has good solubility in different solvent compositions and can be formed into a phosphonate type ion exchange membrane by drying the solution. This good solubility is also conducive to mixing the phosphonate polymer with other materials in the solution to prepare a composite and an ion exchange membrane.

[0210] The conductivity of PEM-7 at 80°C and 95% relative humidity is 0.5 mS / cm.

[0211] Example 8 Preparation of PEM-11

[0212] Weigh 0.5g of PPS-1A in Example 6 and add it to 95g of D1020 resin dispersion (Chemours, perfluorosulfonic acid resin mass content of 10%, EW of 980g / mol, solvent is a mixed solvent of water, ethanol and n-propanol), stir and mix at room temperature for 24h to fully dissolve and disperse PPS-1A. Apply the mixed dispersion on the release film with a scraper, dry at 80°C for 1h, and heat treat at 150°C for 15min to obtain an ion exchange membrane PEM-11 with an average thickness of 50μm.

[0213] The EW of D1020 resin is 980g / mol, and its chemical structure is:

[0214]

[0215] Example 9 Preparation of PEM-21

[0216] Different from Example 8, the amount of PPS-1A added was 5 g, and an ion exchange membrane PEM-21 with an average thickness of 60 μm was obtained. PPS-1A was fully dissolved and dispersed in the dispersion, and the IEC of PEM-21 was 1.21 mmol / g.

[0217] Example 10 Preparation of PEM-31

[0218] Different from Example 8, the amount of PPS-1A added was 9.5 mg, and an ion exchange membrane PEM-31 with an average thickness of 50 μm was obtained. The ion exchange capacity of PEM-31 was 1.02 mmol / g.

[0219] Example 11 Preparation of PEM-13

[0220] 0.5 g of PPS-3 in Example 6 and 0.5 g of PFIA resin were weighed and dissolved in 9 mL of DMF to form a dispersion. The dispersion was cast into an ultra-flat petri dish, dried at 60° C. for 12 h, and heat treated at 120° C. for 15 min to obtain an ion exchange membrane PEM-13 with an average thickness of 200 μm. The IEC of PEM-13 was 1.96 mmol / g.

[0221] The EW of PFIA resin is 625 g / mol and its chemical structure is:

[0222]

[0223] Example 12 Preparation of PEM-14

[0224] 1.2 g of PPS-4 in Example 6 and 8.8 g of Aquivion resin were weighed and dissolved in 40 mL of a water-alcohol mixed solvent (the mass ratio of water, ethanol, and isopropanol was 4:1:5) to form a dispersion. The dispersion was coated on both sides of a polytetrafluoroethylene microporous membrane (thickness 8-10 μm, porosity 76%, pore size distribution 190-280 nm) by a scraper, dried at 90° C. for 5 min, and heat treated at 180° C. for 15 min to obtain an ion exchange membrane PEM-14 with an average thickness of 12 μm.

[0225] The EW of Aquivion resin is 720 g / mol and its chemical structure is:

[0226]

[0227] Example 13 Preparation of PEM-15

[0228] The difference from Example 12 is that the phosphonated polymer is PPS-5, and the obtained ion exchange membrane PEM-15 has an average thickness of 12 μm.

[0229] Example 14 Preparation of PEM-16

[0230] 0.01 g of PPS-6 in Example 6 and 9.99 g of 3M resin were weighed and dissolved in 100 mL of DMF to form a dispersion, 1 mL of the dispersion was cast in an ultra-flat petri dish, and dried at 80° C. for 12 h to obtain an ion exchange membrane PEM-16 with an average thickness of 5 μm. The IEC of PEM-16 is 1.24 mmol / g.

[0231] 3M resin EW is 800g / mol, and its chemical structure is:

[0232]

[0233] Example 15 Preparation of PEM-17

[0234] 9.9 g of PPS-7 in Example 6 and 0.1 g of sulfonated polytrifluorostyrene were weighed and dissolved in 190 mL of a mixed solvent of toluene and n-hexanol (the volume ratio of toluene to n-hexanol was 80:20) to form a dispersion. The dispersion was cast into an ultra-flat petri dish, dried at 100° C. for 6 h, and heat treated at 160° C. for 30 min to obtain an ion exchange membrane PEM-17 with an average thickness of 100 μm. The IEC of PEM-17 is 2.07 mmol / g.

[0235] The EW of sulfonated polytrifluorostyrene is 407 g / mol, and its chemical structure is:

[0236]

[0237] The conductivity of PEM-17 at 80°C and 95% relative humidity is 3.6 mS / cm. The mass content of sulfonated polymer in the ion exchange membrane composed of the composite is only 1%, but compared with PEM-7, the conductivity is significantly increased, and the synergistic effect of phosphonic acid and sulfonic acid functional groups on ion transport is obvious.

[0238] Example 16 Preparation of PEM-27

[0239] Different from Example 15, the addition amount of PPS-7 and sulfonated polytrifluorostyrene is 5 g, and the ion exchange membrane PEM-27 with an average thickness of 100 μm is obtained. The solution obtained by mixing the two polymers is clear and transparent, and the film forming quality is high.

[0240] Example 17 Preparation of PEM-19

[0241] Weigh 1g of PPS-9 in Example 6 and 9g of 3M resin in Example 14 and dissolve them in 40mL of a water-alcohol mixed solvent (the mass ratio of water, ethanol, and n-propanol is 4:4:2) to form a dispersion. The dispersion is applied on both sides of a polytetrafluoroethylene microporous membrane (thickness 15-19 μm, porosity 78%, pore size distribution 240-320 nm) by a scraper, dried at 80°C for 5min, and heat treated at 150°C for 10min to obtain an ion exchange membrane PEM-19 with an average thickness of 25 μm.

[0242] Comparative Example 1

[0243] Weigh 0.5 g of the chloromethylated styrene polymer in Example 3 or 0.5 g of poly (4-bromostyrene), dissolve in 10 mL of carbitol, add 2.5 mL of triethyl phosphite, and react at 155° C. for 24 h to obtain a second phosphonated polymer. Heat the second phosphonated polymer under reflux in a 6 mol / L hydrochloric acid solution for 12 h to obtain a third phosphonated polymer.

[0244] Table 7 shows the reaction materials and structural formulas of the second phosphonated polymer and the third phosphonated polymer. The ion exchange capacity of the second phosphonated polymer is negligible, and the EW of the third phosphonated polymer is shown in Table 7. In the structural formula, R 10 is -CH2CH3, R of the third phosphonated polymer 10 For H.

[0245] Table 7

[0246]

[0247]

[0248] The solubility of the second phosphonated polymer is similar to that of the phosphonated polymer in Example 6, but the solubility of the third phosphonated polymer is poor. PA-3 and PA-4 are partially soluble in DMF, DMAC and DMSO; PA-4 and PA-9 are partially soluble in a mixed solvent of water, ethanol and isopropanol. PA-1 and PA-7 are poorly soluble in any of the solvent combinations listed in Example 7. The poor solubility limits the processing and application of the third phosphonated polymer.

[0249] Comparative Example 2

[0250] Different from Example 8, the phosphonated polymer PPS-1A was not added, and an ion exchange membrane D-PEM-11 with an average thickness of 50 μm was obtained.

[0251] Comparative Example 3

[0252] Different from Example 12, the phosphonated polymer PPS-4 was not added, and an ion exchange membrane D-PEM-14 with an average thickness of 12 μm was obtained.

[0253] Comparative Example 4

[0254] 1.2 g of PA-4 and PA-9 in Comparative Example 1 were dissolved in 12 mL of a water-alcohol solvent to form a phosphonic acid polymer solution. 8.8 g of the Aquivion resin in Example 12 was dissolved in 28 mL of a water-alcohol solvent to form a perfluorosulfonic acid resin solution. The mass ratio of water, ethanol, and isopropanol in the water-alcohol solvent was 4:1:5. The PA-4 solution and the PA-9 solution were mixed with the perfluorosulfonic acid resin solution respectively. After mixing, the solution became turbid. After stirring and standing, a certain amount of polymer solids precipitated and could not be further processed and formed.

[0255] Comparative Example 5

[0256] Different from Example 16, the second phosphonated polymer PE-7 in Comparative Example 1 was mixed with the sulfonated polytrifluorostyrene to produce an ion exchange membrane D-PEM-27 with an average thickness of 100 μm.

[0257] Comparative Example 6

[0258] Different from Example 17, the phosphonated polymer PPS-9 was not added, and an ion exchange membrane D-PEM-19 with an average thickness of 25 μm was obtained.

[0259] Table 8 shows the IEC, water absorption, tensile strength and free radical resistance of the ion exchange membrane.

[0260] Table 8

[0261]

[0262] The IEC and water absorption of the ion exchange membrane containing the phosphonated polymer decrease due to ionic crosslinking, and the reduction in water absorption improves the dimensional stability of the material; the ionic crosslinking also improves the tensile strength and free radical resistance of the ion exchange membrane, which is beneficial to the further processing and application of the membrane material.

[0263] The dual ion transport channels of phosphonic acid groups and sulfonic acid groups improve the conductivity of the ion exchange membrane at different humidity levels, especially at low humidity, the stronger water retention of the phosphonic acid groups is conducive to the transport of protons; as the strongest physical cross-linking structure, the ionic cross-linking effect formed by phosphonic acid-sulfonic acid causes the oxygen permeability and hydrogen permeation current of PEM-14 and PEM-15 to be significantly reduced compared with D-PEM-14, and the barrier property of the ion exchange membrane to oxygen and hydrogen on both sides of the electrode is improved, which can effectively improve the service life and safety of the ion exchange membrane in the fuel cell.

[0264] Table 9 shows the conductivity (temperature 80°C, 50%, 95% relative humidity), oxygen permeability and hydrogen permeation current of the ion exchange membrane.

[0265] Table 9

[0266]

[0267]

[0268] Table 10 shows the conductivity (temperature is 30°C, immersed in deionized water), ion permeability of the ion exchange membrane, and the single cell coulombic efficiency (CE), voltage efficiency (VE) and energy efficiency (EE) of the flow battery membrane.

[0269] Table 10

[0270]

[0271] When ion exchange membranes are used as flow battery separators, the coulombic efficiency is greatly affected by the barrier properties. The ion cross-linking structure reduces the ion permeability of the ion exchange membrane and improves the coulombic efficiency. The increase in conductivity also improves the voltage efficiency and energy efficiency.

[0272] Figure 1 The cross-sectional SEM images of PEM-14 and D-PEM-14 show that the introduction of phosphonated polymer has little effect on the composite of ion exchange resin and microporous membrane. In the two ion exchange membranes with different components, the composite effect of ion exchange resin and microporous membrane is basically the same, with no significant difference.

[0273] Figure 2 This is a TEM image of ultrathin sections (average thickness of about 40nm) of PEM-15 and D-PEM-14. The lighter color in the image is the bright phase (hydrophobic phase), and the darker color is the dark phase (hydrophilic phase). The bright phase is mainly hydrophobic segments, and the dark phase is hydrophilic segments. After the introduction of the block-structured phosphonated polymer, the microphase separation size of the ion exchange membrane changes, and the size of the dark phase increases, which is beneficial to the continuity of hydrated ion transmission. The block-structured phosphonated polymer has a significant effect on the microphase separation structure of the ion exchange membrane.

[0274] Figure 3 and Figure 4 The single cell polarization curves of PEM-14 and D-PEM-14 are shown in Figure 1. The test temperature is 95°C and the humidity is 10%-50%. PEM-14 has better single cell performance under different humidity conditions. Under 50% relative humidity, the power density of PEM-14 reaches 818.4mW / cm 2 @0.65V, higher than D-PEM-14’s 544.6mW / cm 2 @0.65V.

[0275] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0276] Although the above embodiments have been shown and described, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. Changes, modifications, substitutions and variations of the above embodiments by those of ordinary skill in the art are all within the scope of protection of the present invention.

Claims

1. A phosphonated polymer, characterized in that: The phosphonated polymer comprises a repeating unit A0 represented by formula (1): Wherein, R2 is selected from H or F; R3 is selected from H, F or CH3; d is an integer selected from 0 to 12; R4 is at least one selected from H, a C1-C6 alkyl group or an alkali metal.

2. The phosphonated polymer according to claim 1, characterized in that The phosphonated polymer further comprises repeating units A1: Wherein, R2 is selected from H or F; R3 is selected from H, F or CH3; R6 is selected from H, Cl~C 12 Alkyl, C1-C6 perfluoroalkyl or C6-C 12 At least one of the aromatic groups; And / or, the phosphonated polymer further comprises a repeating unit A2, wherein the repeating unit A2 comprises At least one of -CH2CH2-, -CH(CH3)CH2-, -CH(CH2CH3)CH2- or -C(CH3)2CH2-; And / or, the phosphonated polymer further comprises a repeating unit A3: Wherein, R2 is selected from H or F; R3 is selected from H, F or CH3; d is selected from an integer of 0 to 12.

3. The phosphonated polymer according to claim 1, characterized in that The phosphonation degree of the phosphonated polymer is defined as the molar percentage of the repeating unit A0 in all the repeating units containing a benzene ring in the phosphonated polymer; the phosphonation degree is ≥ 0.1%; and / or, the M of the phosphonated polymer n 30,000 to 1,200,000; and / or, the M of the phosphonated polymer w 30,000 to 1,600,000; And / or, the EW of the phosphonated polymer is 216 to 5000 g / mol.

4. A method for preparing the phosphonated polymer according to any one of claims 1 to 3, characterized in that: include: The hydroxyl functional polymer is subjected to a phosphonation reaction with a phosphonating agent to obtain a phosphonated polymer.

5. The method for preparing a phosphonated polymer according to claim 4, characterized in that: The hydroxyl-functionalized polymer is a hydroxyl-functionalized styrene polymer; And / or, the phosphonating agent includes at least one of orthophosphoric acid, oligophosphoric acid with a degree of polymerization less than 10 and its salt, sodium hexametaphosphate, phosphorus trichloride, phosphorus pentachloride, phosphorus oxychloride, and phosphite triester compounds; and / or, the mass ratio of the hydroxyl functionalized polymer to the phosphonating agent is 1:0.2-10; And / or, the temperature of the phosphonation reaction is 20-180°C; And / or, the phosphonation reaction time is 1 min-24 h.

6. The method for preparing a phosphonated polymer according to claim 5, characterized in that: The phosphonating agent includes orthophosphoric acid, and the hydroxyl functionalized polymer and the phosphonating agent are subjected to a phosphonating reaction under the action of a catalyst to obtain a phosphonated polymer.

7. The method for preparing a phosphonated polymer according to claim 6, characterized in that: The catalyst comprises at least one of urea, urea derivatives, guanidine, guanidine derivatives or C3-C6 amines; And / or, the mass ratio of the hydroxyl functionalized polymer to the catalyst is 1:0.2-15.

8. A multifunctional complex, characterized in that: The invention comprises a phosphonated polymer and a sulfonated polymer, wherein the phosphonated polymer comprises the phosphonated polymer described in any one of claims 1 to 3 or the phosphonated polymer prepared by the preparation method described in any one of claims 4 to 7.

9. The multifunctional complex according to claim 8, characterized in that: The invention comprises, by mass, 0.1% to 99.9% of a phosphonated polymer and 0.1% to 99.9% of a sulfonated polymer; And / or, the sulfonated polymer includes at least one of perfluorosulfonic acid resin, polyacid side chain perfluoro resin, sulfonated polytrifluorostyrene, sulfonated polysulfone, sulfonated polyethersulfone, sulfonated polyetheretherketone, sulfonated polyaryletherketone, sulfonated polyarylethernitrile, sulfonated polyphosphazene, sulfonated polyphenylene oxide, sulfonated polybenzonitrile, sulfonated polyimide or sulfonated polybenzimidazole.

10. A method for preparing the multifunctional complex according to claim 8 or 9, characterized in that: include: dispersing the phosphonated polymer and the sulfonated polymer in a solvent to obtain a dispersion; The dispersion is dried to obtain a multifunctional complex.

11. An ion exchange membrane, characterized in that: The invention comprises the phosphonated polymer according to any one of claims 1 to 3 or the multifunctional complex according to claim 8 or 9.

12. The ion exchange membrane according to claim 11, characterized in that The thickness of the ion exchange membrane is 3 to 500 μm; and / or, the ion exchange capacity of the ion exchange membrane is 0.1 to 6.2 mmol / g; And / or, the ion exchange membrane further comprises a porous reinforced membrane; the phosphonated polymer or multi-functional complex is supported on the porous reinforced membrane.

13. A method for preparing an ion exchange membrane according to claim 11 or 12, characterized in that: include: The phosphonated polymer is dispersed in a solvent, or the phosphonated polymer and the sulfonated polymer are dispersed in a solvent, or the multifunctional complex is dispersed in a solvent to obtain a dispersion; the dispersion is subjected to film formation and drying to obtain an ion exchange membrane.

14. Use of the phosphonated polymer according to any one of claims 1 to 3, the multifunctional complex according to claim 8 or 9, or the ion exchange membrane according to claim 11 or 12, characterized in that: Used in at least one of batteries, water electrolysis hydrogen production equipment, chlor-alkali industry, electrodialysis, osmosis, sensors, and supercapacitors.