Macromolecule-based pressure response label paper and preparation method thereof

By synthesizing and polymerizing liquid crystal and piezochromic monomers for label paper, the method addresses dispersion and solubility issues of traditional materials, enabling effective pressure-induced color and luminescent changes.

CN119060246APending Publication Date: 2024-12-03DONGGUAN DANGNA PRINTING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411345454.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing pressure-sensitive intelligent response materials, such as organic and inorganic crystal materials, suffer from poor dispersion and solubility in ink, leading to uneven color or luminescence and loss of pressure response function when dissolved.

Method used

A method is developed to prepare a polymer-based pressure-responsive label paper by synthesizing liquid crystal monomers and piezochromic monomers, then polymerizing them to form a piezochromic polymer material, which is applied to label paper through screen printing.

Benefits of technology

The method achieves dual responses of pressure-induced color change and luminescence, overcoming the limitations of traditional crystal materials by ensuring uniform dispersion and maintaining pressure response functionality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060246A_ABST
    Figure CN119060246A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of macromolecule-based pressure response label paper. The preparation method specifically comprises the following steps: step 1, preparing a liquid crystal monomer; step 2, preparing a piezochromic monomer; step 3, preparing a piezochromic high polymer material according to products obtained in the step 1 and the step 2; and 4, preparing the label paper according to the product obtained in the step 3. The invention also discloses polymer-based pressure response label paper, the pressure response liquid crystal material is prepared, the material is applied to the label paper, and dual responses of piezochromism and luminescence are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of pressure-induced chromatic polymer materials, and relates to a polymer-based pressure-responsive label paper. The invention also relates to a method for preparing the polymer-based pressure-responsive label paper. Background Art

[0002] With the development of social economy and science and technology, various new commodities are increasing, and the use of label paper provides convenience for commodity classification and address positioning. In recent years, high-value commodities are usually given functionality in label paper, such as personalized luminescence and color change.

[0003] When the label paper responds to changes in the external environment such as temperature, pH, light, pressure, electric field strength, magnetic field strength, ionic strength or additive concentration, the microscopic molecular structure or conformation of the functional material changes, thereby showing external detectable or identifiable macroscopic property changes. Piezochromism relies on the complementary colors seen by the human eye after the material absorbs natural light, while piezoluminescence is the color change of the material's luminescent color, resulting in the need to effectively avoid mutual interference when piezochromism and piezoluminescence exist at the same time. The development of smart label paper with piezochromism and piezoluminescence has great potential for application in high-level anti-counterfeiting and personalized products.

[0004] To date, most pressure-sensitive intelligent response materials are aggregated single crystal or polycrystalline materials, such as organic crystal materials, inorganic crystal materials, metal organic framework crystal materials MOFs, etc., which are widely reported. The common method is to add the above-mentioned optical functional crystal materials into ink. However, the particle size of luminescent and color-changing crystal materials is large, and the dispersion and solubility in ink are poor, and the color or luminescence is uneven, which limits their use. The dissolution of crystal materials in ink will cause the material to lose its pressure response function. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a polymer-based pressure-responsive label paper, by which a pressure-responsive liquid crystal material is prepared, and the material is applied to the label paper to achieve dual responses of pressure-induced color change and luminescence.

[0006] Another object of the present invention is to provide a polymer-based pressure-responsive label paper.

[0007] The technical solution adopted by the present invention is a method for preparing a polymer-based pressure-responsive label paper, which specifically comprises the following steps:

[0008] Step 1, preparing liquid crystal monomers;

[0009] Step 2, preparing a piezochromic monomer;

[0010] Step 3, preparing a piezochromic polymer material according to the products obtained in step 1 and step 2;

[0011] Step 4, preparing label paper according to the product obtained in step 3.

[0012] The present invention is also characterized in that:

[0013] The specific process of step 1 is:

[0014] Step 1.1, 1.36 g to 4.08 g of p-hydroxybenzoic acid and 2.64 g to 7.92 g of 12-bromo-1-dodecanol are added to 20 mL to 60 mL of ethanol solution, and then 0.1 g to 0.3 g of sodium ethoxide is added, and the mixture is refluxed at 80° C. to 100° C. for 12 h to 24 h. After the reaction is completed, the mixture is rotary evaporated at 45-60° C., and column separation is performed to obtain intermediate product I;

[0015] Step 1.2, dissolving the intermediate product I in 20 mL to 60 mL of N-methylpyrrolidone solvent, then adding 1 mL to 3 mL of acryloyl chloride to react at room temperature for 5 h, and performing rotary evaporation at 45-60 ° C and column separation to obtain the intermediate product II;

[0016] Step 1.3, dissolve the intermediate product II in 30mL-90mL chloroform solvent, then add 3.2g-9.6g of 4-hydroxybenzonitrile and 2.06g-6.18g of dehydrating agent N,N-dicyclohexylcarbodiimide respectively, react at room temperature for 20h-40h, and obtain liquid crystal monomer by column separation.

[0017] The specific process of step 2 is:

[0018] Step 2.1, add 1.36 g to 4.08 g of p-hydroxybenzoic acid and 1.52 g to 4.56 g of 4-vinylbenzyl chloride to 10 mL to 30 mL of N, N-dimethylformamide solution, and then add 0.3 g to 0.9 g of NaCO 3 , stirring at 50°C to 70°C for 12h to 24h, after the reaction is completed and cooled to room temperature, the cooled solution is poured into 100mL to 300mL of ice water, washed three times with 100mL to 300mL of deionized water, and a pale white solid is collected to obtain product A;

[0019] Step 2.2, 3.35 g to 10.05 g of triphenylethylene bromide and 1.79 g to 5.37 g of 4-carbomethoxyphenylboronic acid are dissolved in 20 mL to 60 mL of toluene solvent, 0.1 g to 0.3 g of Pd(0) catalyst and 0.5 g to 1.5 g of potassium carbonate are added, and the reaction is carried out for 12 h to 24 h under nitrogen protection. After cooling, the product B is obtained by rotary evaporation at 45-60 ° C and column separation;

[0020] Step 2.3, take 0.5g-1.5g of product A and 0.8g-2.4g of product B, dissolve them in 20mL-60mL of tetrahydrofuran solvent, add 0.2g-0.6g of sodium ethoxide and react at 45℃-60℃ for 4-6h, after the reaction is completed, cool and evaporate at 45-60℃, and separate by column to obtain product C;

[0021] Step 2.4, take 1.95g-3.9g of product C and 0.33-0.66g of boron trifluoride dimethyl ether, add 10mL-30mL of tetrahydrofuran, heat at 45°C-60°C to react for 5h-10h, cool and dry, and separate the piezochromic monomer by column.

[0022] The specific process of step 3 is:

[0023] Take 1g to 2g of liquid crystal monomer and 0.08g to 0.16g of piezochromic monomer, dissolve them in 5mL to 10mL of N,N-dimethylformamide solution, add 0.02g to 0.06g of azobisisobutyronitrile catalyst, heat to 90℃ to 110℃ and react for 12h to 18h. After the reaction, introduce the reaction solution into 100mL to 200mL of industrial alcohol, collect the precipitated product, dry it at 45℃ to 60℃ for 24h to 48h, and set it aside.

[0024] The specific process of step 4 is: take 0.5g~1g of piezochromic polymer and dissolve it in 3mL~6mL of DMSO solvent, let it stand at room temperature for 24~48h, self-assemble to form a piezochromic liquid crystal mobile phase, take a 10cmx10cm label paper base paper, and print the piezochromic liquid crystal mobile phase on the label paper base paper by screen printing, with a thickness of 60um~120um, and dry it at 80℃~100℃ for 8h~12h to obtain pressure-responsive label paper.

[0025] The second technical solution adopted by the present invention is a polymer-based pressure-responsive label paper, which is prepared by adopting the above-mentioned method for preparing the polymer-based pressure-responsive label paper.

[0026] The beneficial effect of the present invention is that the present invention adopts polymerization to covalently bond pressure-responsive molecules to liquid crystal polymers to achieve pressure-induced color and luminescent color changes. Pressure-responsive molecules are covalently bonded to liquid crystal polymers by polymerization, and used for smart label paper. Under the action of curling, the response performance of the label paper is adjusted, including the dual changes of its own color and luminescent color. The problem that traditional crystal materials cannot be used in ink due to large particles and the failure of pressure-responsive performance after dissolution is well solved. The prepared liquid crystal material can realize the ink function through screen printing. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1It is a fluorescence spectrum diagram of the label paper prepared in Example 1 and Comparative Examples 2 and 3 in the method for preparing a polymer-based pressure-responsive label paper of the present invention. DETAILED DESCRIPTION

[0028] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0029] The present invention provides a method for preparing a polymer-based pressure-responsive label paper, which specifically comprises the following steps:

[0030] Step 1, synthesizing liquid crystal monomers, specifically:

[0031] 1.36-4.08g of p-hydroxybenzoic acid and 2.64-7.92g of 12-bromo-1-dodecanol are added to 20-60mL of ethanol solution, and then 0.1-0.3g of sodium ethoxide is added, and the reaction is refluxed at 80-100℃ for 12-24h. After the reaction is completed, the reaction is rotary evaporated at 45-60℃, and the intermediate product I is obtained by column separation. The intermediate product I is dissolved in 20-60mL of N-methylpyrrolidone solvent, and then 1-3mL of acryloyl chloride is added to react at room temperature for 5h, and the intermediate product II is obtained by rotary evaporation and column separation at 45-60℃; the intermediate product II is dissolved in 30-90mL of chloroform solvent, 3.2-9.6g of 4-hydroxybenzonitrile and 2.06-6.18g of dehydrating agent N,N-dicyclohexylcarbodiimide are added, and the reaction is carried out at room temperature for 20-40h, and the liquid crystal monomer is obtained by column separation.

[0032] Step 2, synthesizing a piezochromic monomer, specifically:

[0033] Take 1.36-4.08g of p-hydroxybenzoic acid and 1.52-4.56g of 4-vinylbenzyl chloride and add them to 10-30mL of N,N-dimethylformamide solution, then add 0.3-0.9g of NaCO 3, stirring at 50-70℃ for 12-24h. After the reaction is completed and cooled to room temperature, the cooled solution is poured into 100-300mL ice water, washed 3 times with 100-300mL deionized water, and the pale white solid is collected to obtain product A; 3.35-10.05g of triphenylethylene bromide and 1.79-5.37g of 4-methyl ester phenylboronic acid are dissolved in 20-60mL of toluene solvent, 0.1-0.3g of Pd(0) catalyst and 0.5-1.5g of potassium carbonate are added, and the reaction is carried out under nitrogen protection for 12-24h. After cooling, the product B is obtained by rotary evaporation and column separation at 45-60℃; 0.5-1.5g of product A and 0.8-2.4g of product B are taken, dissolved in 20-60mL of tetrahydrofuran solvent, and 0.2-0.6g of sodium ethoxide is added and reacted at 45-60℃ for 4-6h. After the reaction is completed, the mixture is cooled and subjected to rotary evaporation at 45-60°C, and the product C is separated by column. 1.95-3.9 g of the product C and 0.33-0.66 g of boron trifluoride dimethyl ether are added with 10-30 mL of tetrahydrofuran, and the mixture is heated at 45-60°C for reaction for 5-10 h, cooled and dried at 45-60°C for 12 h, and the pressure-induced chromic monomer is separated by column.

[0034] Step 3, synthesizing a pressure-induced chromic polymer material, specifically:

[0035] Take 1-2g of liquid crystal monomer and 0.08-0.16g of piezochromic monomer, dissolve in 5-10mL of N,N-dimethylformamide solution, add 0.02-0.06g of azobisisobutyronitrile catalyst, heat to 90-110℃ and react for 12-18h. After the reaction is completed, introduce the reaction solution into 100-200mL of industrial alcohol, collect the precipitated product, dry it at 45-60℃ for 24-48h, and set aside.

[0036] Step 4, preparation of label paper, specifically:

[0037] Take 0.5-1g of piezochromic polymer and dissolve it in 3-6mL of DMSO (dimethyl sulfoxide) solvent, let it stand at room temperature for 24-48h to self-assemble to form a piezochromic liquid crystal mobile phase, take a 10cmx10cm label paper base paper, print the piezochromic liquid crystal mobile phase on the label paper base paper by screen printing, with a thickness of 60-120um, and dry it at 80-100℃ for 8-12h to obtain a pressure-responsive label paper.

[0038] Example 1

[0039] Step 1, synthesizing liquid crystal monomers, specifically:

[0040] Take 1.36g of p-hydroxybenzoic acid and 2.64g of 12-bromo-1-dodecanol and add them to 20mL of ethanol solution, then add 0.1g of sodium ethoxide and reflux at 80℃ for 12h. After the reaction is completed, perform rotary evaporation at 60℃ and column separation to obtain intermediate product I. Dissolve intermediate product I in 20mL of N-methylpyrrolidone solvent, then add 1mL of acryloyl chloride and react at room temperature for 5h, and perform rotary evaporation and column separation at 60℃ to obtain intermediate product II. Dissolve intermediate product II in 30mL of chloroform solvent, add 3.2g of 4-hydroxybenzonitrile and 2.06g of dehydrating agent N,N-dicyclohexylcarbodiimide, react at room temperature for 20h, and obtain liquid crystal monomer by column separation.

[0041] Step 2, synthesizing a piezochromic monomer, specifically:

[0042] Take 1.36 g of p-hydroxybenzoic acid and 1.52 g of 4-vinylbenzyl chloride and add them to 10 mL of N,N-dimethylformamide solution, then add 0.3 g of NaCO 3 , stir at 50℃ for 12-24h. After the reaction is completed and cooled to room temperature, pour the cooled solution into 100mL of ice water, wash 3 times with 100mL of deionized water, collect the pale white solid, and obtain product A; take 3.35g of triphenylethylene bromide and 1.79g of 4-methyl ester phenylboronic acid and dissolve them in 20mL of toluene solvent, add 0.1g of Pd(0) catalyst and 0.5g of potassium carbonate, and react for 12h under nitrogen protection. After cooling, 60℃ rotary evaporation and column separation are obtained to obtain product B; take 0.5g of product A and 0.8g of product B, dissolve them in 20mL of tetrahydrofuran solvent, add 0.2g of sodium ethoxide and react at 45℃ for 4h. After the reaction is completed, cool and 60℃ rotary evaporation, column separation is obtained to obtain product C. Take 1.95 g of product C and 0.33 g of boron trifluoride dimethyl ether, add 10 mL of tetrahydrofuran, heat to 45° C. for 5 h, cool and dry at 45° C. for 12 h, and separate the piezochromic monomer by column.

[0043] Step 3, synthesizing a pressure-induced chromic polymer material, specifically:

[0044] Take 1g of liquid crystal monomer and 0.08g of piezochromic monomer, dissolve in 5mL of N,N-dimethylformamide solution, add 0.02g of azobisisobutyronitrile catalyst, and heat to 90℃ for 12h. After the reaction, introduce the reaction solution into 100mL of industrial alcohol, collect the precipitated product, and dry it at 45℃ for 24h for later use.

[0045] 3.4 Preparation of pressure-responsive label paper

[0046] Take 0.5g of piezochromic polymer and dissolve it in 3mL of DMSO solvent. Let it stand at room temperature for 24h to self-assemble into a piezochromic liquid crystal mobile phase. Take a 10cmx10cm label paper base paper and print the piezochromic liquid crystal mobile phase on the label paper base paper by screen printing with a thickness of 60um. Dry it at 80℃ for 8h to obtain the pressure-responsive label paper.

[0047] Comparative Example 1 (liquid crystal monomer and pressure-induced chromatic monomer were not polymerized, label paper was directly screen-printed, film could not be formed, and there was no pressure-induced color change)

[0048] Step 1, synthesis of liquid crystal monomers, specifically:

[0049] 1.36 g of p-hydroxybenzoic acid and 2.64 g of 12-bromo-1-dodecanol were added to 20 mL of ethanol solution, and then 0.1 g of sodium ethoxide was added, and the mixture was refluxed at 80°C for 12 h. After the reaction was completed, the reaction was performed by rotary evaporation at 60°C and column separation to obtain intermediate product I. The intermediate product I was dissolved in 20 mL of N-methylpyrrolidone solvent, and then 1 mL of acryloyl chloride was added to react at room temperature for 5 h. The intermediate product II was obtained by rotary evaporation and column separation at 60°C. The intermediate product II was dissolved in 30 mL of chloroform solvent, and 3.2 g of 4-hydroxybenzonitrile and 2.06 g of dehydrating agent N,N-dicyclohexylcarbodiimide were added, and the mixture was reacted at room temperature for 20 h. The liquid crystal monomer was obtained by column separation.

[0050] Step 2, synthesis of the piezochromic monomer, specifically:

[0051] Take 1.36 g of p-hydroxybenzoic acid and 1.52 g of 4-vinylbenzyl chloride and add them to 10 mL of N,N-dimethylformamide solution, then add 0.3 g of NaCO 3 , stir at 50℃ for 12-24h. After the reaction is completed and cooled to room temperature, pour the cooled solution into 100mL of ice water, wash 3 times with 100mL of deionized water, collect the pale white solid, and name it product A; take 3.35g of triphenylethylene bromide and 1.79g of 4-methyl ester phenylboronic acid and dissolve them in 20mL of toluene solvent, add 0.1g of Pd(0) catalyst and 0.5g of potassium carbonate, and react for 12h under nitrogen protection. After cooling, 60℃ rotary evaporation and column separation give product B; take 0.5g of product A and 0.8g of product B, dissolve them in 20mL of tetrahydrofuran solvent, add 0.2g of sodium ethoxide and react at 45℃ for 4h. After the reaction is completed, cool and 60℃ rotary evaporation, column separation give product C. Take 1.95 g of product C and 0.33 g of boron trifluoride dimethyl ether, add 10 mL of tetrahydrofuran, heat to 45° C. for 5 h, cool and dry at 60° C. for 12 h, and separate the piezochromic monomer by column.

[0052] Step 3, preparation of pressure-responsive label paper, specifically:

[0053] Take 5g of liquid crystal monomer and 0.04g of piezochromic monomer and dissolve them in 3mL of DMSO solvent. Let them stand at room temperature for 24h to self-assemble into a piezochromic liquid crystal mobile phase. Take a 10cmx10cm label paper base paper and print the piezochromic liquid crystal mobile phase on the label paper base paper by screen printing with a thickness of 60um. Dry at 80℃ for 8h to obtain pressure-responsive label paper.

[0054] Comparative Example 2 (When polymer materials are polymerized, no piezochromic monomer is added, the color change is narrow, and there is no change in the piezoluminescent color)

[0055] Step 1, synthesis of liquid crystal monomers, specifically:

[0056] 1.36 g of p-hydroxybenzoic acid and 2.64 g of 12-bromo-1-dodecanol were added to 20 mL of ethanol solution, and then 0.1 g of sodium ethoxide was added, and the mixture was refluxed at 80°C for 12 h. After the reaction was completed, the reaction was performed by rotary evaporation at 60°C and column separation to obtain intermediate product I. The intermediate product I was dissolved in 20 mL of N-methylpyrrolidone solvent, and then 1 mL of acryloyl chloride was added to react at room temperature for 5 h. The intermediate product II was obtained by rotary evaporation and column separation at 60°C. The intermediate product II was dissolved in 30 mL of chloroform solvent, and 3.2 g of 4-hydroxybenzonitrile and 2.06 g of dehydrating agent N,N-dicyclohexylcarbodiimide were added, and the mixture was reacted at room temperature for 20 h. The liquid crystal monomer was obtained by column separation.

[0057] Step 2, synthesis of liquid crystal polymer materials, specifically:

[0058] Take 1g of liquid crystal monomer and dissolve it in 5mL of N,N-dimethylformamide solution, add 0.02g of azobisisobutyronitrile catalyst, and heat to 90℃ for 12h. After the reaction, introduce the reaction solution into 100mL of industrial alcohol, collect the precipitated product, and dry it at 45℃ for 24h for later use.

[0059] Step 3, preparation of pressure-responsive label paper, specifically:

[0060] Take 0.5g of liquid crystal polymer and dissolve it in 3mL of DMSO solvent. Let it stand at room temperature for 24h to self-assemble to form a piezochromic liquid crystal mobile phase. Take a 10cmx10cm label paper base paper and print the piezochromic liquid crystal mobile phase on the label paper base paper by screen printing with a thickness of 60um. Dry it at 80℃ for 8h to obtain a pressure-responsive label paper.

[0061] Comparative Example 3 (no pressure-induced chromic monomer is added during polymer polymerization, and the pressure-induced chromic monomer is physically compounded with the liquid crystal polymer during the preparation of the pressure-responsive label paper, and the pressure-induced color change range is narrow and there is no pressure-induced luminescent color change)

[0062] Step 1, synthesis of liquid crystal monomers, specifically:

[0063] 1.36 g of p-hydroxybenzoic acid and 2.64 g of 12-bromo-1-dodecanol were added to 20 mL of ethanol solution, and then 0.1 g of sodium ethoxide was added, and the mixture was refluxed at 80°C for 12 h. After the reaction was completed, the reaction was performed by rotary evaporation at 60°C and column separation to obtain intermediate product I. The intermediate product I was dissolved in 20 mL of N-methylpyrrolidone solvent, and then 1 mL of acryloyl chloride was added to react at room temperature for 5 h. The intermediate product II was obtained by rotary evaporation and column separation at 60°C. The intermediate product II was dissolved in 30 mL of chloroform solvent, and 3.2 g of 4-hydroxybenzonitrile and 2.06 g of dehydrating agent N,N-dicyclohexylcarbodiimide were added, and the mixture was reacted at room temperature for 20 h. The liquid crystal monomer was obtained by column separation.

[0064] Step 2, synthesis of the piezochromic monomer, specifically:

[0065] Take 1.36 g of p-hydroxybenzoic acid and 1.52 g of 4-vinylbenzyl chloride and add them to 10 mL of N,N-dimethylformamide solution, then add 0.3 g of NaCO 3 , stirred at 50℃ for 12h. After the reaction is completed and cooled to room temperature, the cooled solution is poured into 100mL of ice water, washed 3 times with 100mL of deionized water, and the pale white solid is collected and named product A; 3.35g of triphenylethylene bromide and 1.79g of 4-methylbenzene boronic acid are dissolved in 20mL of toluene solvent, 0.1g of Pd(0) catalyst and 0.5g of potassium carbonate are added, and the reaction is carried out for 12h under nitrogen protection. After cooling, the product B is obtained by rotary evaporation at 60℃ and column separation. 0.5g of product A and 0.8g of product B are taken, dissolved in 20mL of tetrahydrofuran solvent, and 0.2g of sodium ethoxide is added at 45° for 4h. After the reaction is completed, the product C is obtained by rotary evaporation at 60℃ and column separation after cooling. Take 1.95 g of product C and 0.33 g of boron trifluoride dimethyl ether, add 10 mL of tetrahydrofuran, heat to 45° C. for 5 h, cool and dry at 60° C. for 12 h, and separate the piezochromic monomer by column.

[0066] Step 3, synthesis of liquid crystal polymer materials, specifically:

[0067] Take 1g of liquid crystal monomer and dissolve it in 5mL of N,N-dimethylformamide solution, add 0.02g of azobisisobutyronitrile catalyst, and heat to 90℃ for 12h. After the reaction, introduce the reaction solution into 100mL of industrial alcohol, collect the precipitated product, and dry it at 45℃ for 24h for later use.

[0068] Step 4, preparation of pressure-responsive label paper, specifically:

[0069] Take 0.5g of liquid crystal polymer and 0.04g of piezochromic monomer and dissolve them in 3mL of DMSO solvent. Let them stand at room temperature for 24h to self-assemble into a piezochromic liquid crystal mobile phase. Take a 10cmx10cm label paper base paper and print the piezochromic liquid crystal mobile phase on the label paper base paper by screen printing with a thickness of 60um. Dry at 80℃ for 8h to obtain pressure-responsive label paper.

[0070] Experimental Results

[0071] Table 1 Color changes and luminescence changes of Example 1 and Comparative Examples 1-3 under the condition of curling radius of 0.5 cm

[0072]

[0073]

[0074] The pressure-induced color change test method is to curl the label paper at a radius of 0.5 cm and observe the color change of the inner side under natural light conditions and the change of the luminous color under 365nm ultraviolet light. The curling force is inversely proportional to the curling radius: F = κ / λ, κ is a constant, λ is the curling radius.

[0075] Since the monomers in Comparative Example 1 are all small molecule monomers, they cannot form a film on the surface of the label paper after screen printing, and the color and luminescence performance cannot be tested.

[0076] The study found that the label paper in Example 1 has a change in the color of the liquid crystal film and the color of the light emission under the action of curling, and has a good response effect to the action of force. Figure 1 As shown, the color change of Example 1 is relatively wide. The main reason is that when the liquid crystal monomer and the piezochromic monomer are polymerized, the liquid crystal monomer content is large to form the main skeleton of the liquid crystal polymer, and the piezochromic monomer content is small as the object. The piezochromic monomer molecules are polymerized and disorderly bonded to the liquid crystal polymer skeleton. The liquid crystal structure and pitch are changed by the curling force, so that the color change range of the pressure-responsive label paper is wide, from blue to yellow, and the maximum reflection wavelength changes from 430 to 550nm. It is worth noting that in Comparative Example 3, although the piezochromic monomer is physically mixed into the liquid crystal polymer, it does not form a strong effect with the liquid crystal polymer. The piezochromic monomer aggregates during the liquid crystal formation process and has little effect on the liquid crystal formation. Therefore, the color changes of Comparative Examples 2-3 are similar and smaller, from blue to cyan, and the maximum reflection wavelength changes from 430 to 480nm.

[0077] Comparative Example 2 has no piezochromic monomer, resulting in no piezoluminescent color change; in Comparative Example 3, the piezochromic monomer is not dispersed in the liquid crystal polymer. The curling cannot form a change in luminescent color, and the luminescent position is fixed at 430nm.

[0078] Example 2

[0079] Step 1, synthesizing liquid crystal monomers, specifically:

[0080] Take 2.28g of p-hydroxybenzoic acid and 5.48g of 12-bromo-1-dodecanol and add them to 40mL of ethanol solution, then add 0.2g of sodium ethoxide and reflux at 90℃ for 18h. After the reaction is completed, perform rotary evaporation at 50℃ and column separation to obtain intermediate product I. Dissolve intermediate product I in 40mL of N-methylpyrrolidone solvent, then add 2mL of acryloyl chloride and react at room temperature for 5h, and perform rotary evaporation and column separation at 50℃ to obtain intermediate product II. Dissolve intermediate product II in 60mL of chloroform solvent, add 4.8g of 4-hydroxybenzonitrile and 4.28g of dehydrating agent N,N-dicyclohexylcarbodiimide, react at room temperature for 30h, and obtain liquid crystal monomer by column separation.

[0081] Step 2, synthesizing a piezochromic monomer, specifically:

[0082] Take 2.28 g of p-hydroxybenzoic acid and 3.48 g of 4-vinylbenzyl chloride and add them to 20 mL of N,N-dimethylformamide solution, then add 0.6 g of NaCO 3 , stirred at 60℃ for 20h. After the reaction is completed and cooled to room temperature, the cooled solution is poured into 200mL of ice water, washed 3 times with 200mL of deionized water, and the pale white solid is collected to obtain product A; 5.68g of triphenylethylene bromide and 4.38g of 4-methylbenzene boronic acid are dissolved in 40mL of toluene solvent, 0.2g of Pd(0) catalyst and 0.8g of potassium carbonate are added, and the reaction is carried out for 20h under nitrogen protection. After cooling, the product B is obtained by rotary evaporation at 50℃ and column separation; 1.2g of product A and 1.8g of product B are dissolved in 40mL of tetrahydrofuran solvent, 0.4g of sodium ethoxide is added, and the reaction is carried out at 50℃ for 5h. After the reaction is completed, the product C is obtained by rotary evaporation at 50℃ and column separation after cooling. Take 2.4 g of product C and 0.48 g of boron trifluoride dimethyl ether, add 20 mL of tetrahydrofuran, heat to 50° C. for reaction for 8 h, cool and dry at 50° C. for 12 h, and separate the pressure-induced chromic monomer by column.

[0083] Step 3, synthesizing a pressure-induced chromic polymer material, specifically:

[0084] Take 1.5g of liquid crystal monomer and 0.12g of piezochromic monomer, dissolve them in 8mL of N,N-dimethylformamide solution, add 0.04g of azobisisobutyronitrile catalyst, and heat to 100℃ for 16h. After the reaction, introduce the reaction solution into 150mL of industrial alcohol, collect the precipitated product, and dry it at 50℃ for 36h for later use.

[0085] Step 4, preparation of pressure-responsive label paper, specifically:

[0086] Take 0.8g of piezochromic polymer and dissolve it in 4mL of DMSO solvent. Let it stand at room temperature for 36h to self-assemble into a piezochromic liquid crystal mobile phase. Take a 10cmx10cm label paper base paper and print the piezochromic liquid crystal mobile phase on the label paper base paper by screen printing with a thickness of 80um. Dry it at 90℃ for 10h to obtain the pressure-responsive label paper.

[0087] Example 3

[0088] Step 1, synthesizing liquid crystal monomers, specifically:

[0089] Take 4.08g of p-hydroxybenzoic acid and 7.92g of 12-bromo-1-dodecanol and add them to 60mL of ethanol solution, then add 0.3g of sodium ethoxide and reflux at 100℃ for 24h. After the reaction is completed, perform rotary evaporation at 60℃ and column separation to obtain intermediate product I. Dissolve intermediate product I in 60mL of N-methylpyrrolidone solvent, then add 3mL of acryloyl chloride and react at room temperature for 5h, and perform rotary evaporation and column separation at 60℃ to obtain intermediate product II. Dissolve intermediate product II in 90mL of chloroform solvent, add 9.6g of 4-hydroxybenzonitrile and 6.18g of dehydrating agent N,N-dicyclohexylcarbodiimide, react at room temperature for 40h, and obtain liquid crystal monomer by column separation.

[0090] Step 2, synthesizing a piezochromic monomer, specifically:

[0091] Take 4.08 g of p-hydroxybenzoic acid and 4.56 g of 4-vinylbenzyl chloride and add them to 30 mL of N,N-dimethylformamide solution, then add 0.9 g of NaCO 3 , stirred at 70℃ for 24h. After the reaction is completed and cooled to room temperature, the cooled solution is poured into 300mL of ice water, washed 3 times with 300mL of deionized water, and the pale white solid is collected to obtain product A; 10.05g of triphenylethylene bromide and 5.37g of 4-methyl ester phenylboronic acid are dissolved in 60mL of toluene solvent, 0.3g of Pd(0) catalyst and 1.5g of potassium carbonate are added, and the reaction is carried out for 24h under nitrogen protection. After cooling, the product B is obtained by rotary evaporation at 45℃ and column separation; 1.5g of product A and 2.4g of product B are taken, dissolved in 60mL of tetrahydrofuran solvent, 0.6g of sodium ethoxide is added, and the reaction is carried out at 60℃ for 6h. After the reaction is completed, the product C is obtained by rotary evaporation at 45℃ and column separation after cooling. Take 3.9 g of product C and 0.66 g of boron trifluoride dimethyl ether, add 30 mL of tetrahydrofuran, heat to 60° C. for 10 h, cool and dry at 60° C. for 12 h, and separate the piezochromic monomer by column.

[0092] Step 3, synthesizing a pressure-induced chromic polymer material, specifically:

[0093] Take 2g of liquid crystal monomer and 0.16g of piezochromic monomer, dissolve them in 10mL of N,N-dimethylformamide solution, add 0.06g of azobisisobutyronitrile catalyst, and heat to 110℃ for 18h. After the reaction, introduce the reaction solution into 200mL of industrial alcohol, collect the precipitated product, and dry it at 60℃ for 48h for later use.

[0094] Step 4, preparation of pressure-responsive label paper, specifically:

[0095] Take 1g of piezochromic polymer and dissolve it in 6mL of DMSO solvent. Let it stand at room temperature for 48h to self-assemble into a piezochromic liquid crystal mobile phase. Take a 10cmx10cm label paper base paper and print the piezochromic liquid crystal mobile phase on the label paper base paper by screen printing with a thickness of 120um. Dry it at 100℃ for 12h to obtain the pressure-responsive label paper.

[0096] The present invention adopts polymerization to covalently bond pressure-induced responsive molecules to liquid crystal polymers to achieve pressure-induced color and luminescent color changes. The piezochromic molecules are covalently bonded to liquid crystal polymers by polymerization, and are used for intelligent pressure-responsive label paper. The pressure-induced responsive performance of the label paper is adjusted by the action of liquid crystal pitch and torque, including the dual change of its own color and luminescent color. The piezochromic and liquid crystal copolymerization is selected, and the dispersion effect of the crystal material in the ink is abandoned.

Claims

1. A method for preparing a polymer-based pressure-responsive label paper, characterized in that: The specific steps include: Step 1, preparing liquid crystal monomers; Step 2, preparing a piezochromic monomer; Step 3, preparing a piezochromic polymer material according to the products obtained in step 1 and step 2; Step 4, preparing label paper according to the product obtained in step 3.

2. The method for preparing a polymer-based pressure-responsive label paper according to claim 1, characterized in that: The specific process of step 1 is as follows: Step 1.1, 1.36 g to 4.08 g of p-hydroxybenzoic acid and 2.64 g to 7.92 g of 12-bromo-1-dodecanol are added to 20 mL to 60 mL of ethanol solution, and then 0.1 g to 0.3 g of sodium ethoxide is added, and the mixture is refluxed at 80° C. to 100° C. for 12 h to 24 h. After the reaction is completed, the mixture is rotary evaporated at 45-60° C., and column separation is performed to obtain intermediate product I; Step 1.2, dissolving the intermediate product I in 20 mL to 60 mL of N-methylpyrrolidone solvent, then adding 1 mL to 3 mL of acryloyl chloride to react at room temperature for 5 h, and performing rotary evaporation at 45-60 ° C and column separation to obtain the intermediate product II; Step 1.3, dissolve the intermediate product II in 30mL-90mL chloroform solvent, then add 3.2g-9.6g of 4-hydroxybenzonitrile and 2.06g-6.18g of dehydrating agent N,N-dicyclohexylcarbodiimide respectively, react at room temperature for 20h-40h, and obtain liquid crystal monomer by column separation.

3. The method for preparing a polymer-based pressure-responsive label paper according to claim 1, characterized in that: The specific process of step 2 is: Step 2.1, add 1.36g to 4.08g of p-hydroxybenzoic acid and 1.52g to 4.56g of 4-vinylbenzyl chloride to 10mL to 30mL of N,N-dimethylformamide solution, then add 0.3g to 0.9g of NaCO3, stir at 50°C to 70°C for 12h to 24h, cool to room temperature after the reaction is completed, pour the cooled solution into 100mL to 300mL of ice water, wash 3 times with 100mL to 300mL of deionized water, collect the pale white solid, and obtain product A; Step 2.2, 3.35 g to 10.05 g of triphenylethylene bromide and 1.79 g to 5.37 g of 4-carbomethoxyphenylboronic acid are dissolved in 20 mL to 60 mL of toluene solvent, 0.1 g to 0.3 g of Pd(0) catalyst and 0.5 g to 1.5 g of potassium carbonate are added, and the reaction is carried out for 12 h to 24 h under nitrogen protection. After cooling, the product B is obtained by rotary evaporation at 45-60 ° C and column separation; Step 2.3, take 0.5g-1.5g of product A and 0.8g-2.4g of product B, dissolve them in 20mL-60mL of tetrahydrofuran solvent, add 0.2g-0.6g of sodium ethoxide and react at 45℃-60℃ for 4-6h, after the reaction is completed, cool and evaporate at 45-60℃, and separate by column to obtain product C; Step 2.4, take 1.95g-3.9g of product C and 0.33-0.66g of boron trifluoride dimethyl ether, add 10mL-30mL of tetrahydrofuran, heat at 45°C-60°C to react for 5h-10h, cool and dry, and separate the piezochromic monomer by column.

4. The method for preparing a polymer-based pressure-responsive label paper according to claim 1, characterized in that: The specific process of step 3 is as follows: Take 1g to 2g of liquid crystal monomer and 0.08g to 0.16g of piezochromic monomer, dissolve them in 5mL to 10mL of N,N-dimethylformamide solution, add 0.02g to 0.06g of azobisisobutyronitrile catalyst, heat to 90℃ to 110℃ and react for 12h to 18h. After the reaction, introduce the reaction solution into 100mL to 200mL of industrial alcohol, collect the precipitated product, dry it at 45℃ to 60℃ for 24h to 48h, and set it aside.

5. The method for preparing a polymer-based pressure-responsive label paper according to claim 1, characterized in that: The specific process of step 4 is as follows: 0.5 g to 1 g of the piezochromic polymer is dissolved in 3 mL to 6 mL of DMSO solvent, and the mixture is allowed to stand at room temperature for 24 to 48 hours to self-assemble into a piezochromic liquid crystal mobile phase. A 10 cm x 10 cm label paper base is taken, and the piezochromic liquid crystal mobile phase is printed on the label paper base by screen printing with a thickness of 60 um to 120 um, and the label paper is dried at 80° C. to 100° C. for 8 hours to 12 hours to obtain a pressure-responsive label paper.

6. A polymer-based pressure-responsive label paper, characterized in that: The label is prepared by the method for preparing a polymer-based pressure-responsive label paper as described in any one of claims 1 to 5.