Preparation method of three-dimensional network structure self-repairing polyurethane with high tensile property and strong adhesion property
Through double cross-linking, the construction of a three-dimensional network structure and the introduction of dynamic covalent bonds is solved, and the problem of insufficient mechanical stretching and adhesion performance of polyurethane materials is achieved, and the polyurethane materials with high tensile and strong adhesion performance is improved, which has improved its durability and application value.
Patent Information
- Application Number
- CN202411329353.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-12-03
AI Technical Summary
The existing polyurethane materials have insufficient mechanical tensile properties and adhesion properties during use, making it difficult to improve their durability and application value.
The three-dimensional network structure is constructed by double cross-linking method, combining siloxane bonds and dynamic covalent bonds, introducing hydrogen bonds and imine bonds, and forming high stretching and strong viscosity through the reaction of phenylene triformaldehyde and polyether polyol. Polyurethane with properties.
It significantly improves the maximum elongation of break and maximum stress of polyurethane, enhances self-healing performance, achieves high tensile and strong adhesion performance, and is suitable for electronic skin and soft robot fields.
Smart Images

Figure CN119060288A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of new materials, and specifically relates to a method for preparing a three-dimensional network structure self-repairing polyurethane with high tensile and strong adhesion properties. Background Art
[0002] Polyurethane is one of the most promising polymer materials. However, due to damage during use, its service life is shortened, resulting in waste that is difficult to recycle and causing many environmental problems. Currently, introducing self-healing functions to improve the durability of polyurethane materials has become an effective way to solve the pollution problem.
[0003] In general, self-healing methods in polyurethane are divided into two types: exogenous and endogenous. Exogenous self-healing methods refer to the addition of microcapsules / microvessels containing healing agents to polymers. Endogenous self-healing methods refer to the introduction of dynamic reversible structures, including dynamic covalent bonds (such as disulfide bonds, Diels-Alder (DA) bonds, imine bonds, and borate bonds) and non-dynamic covalent interactions (such as hydrogen bonds, metal coordination interactions, and host-guest interactions). However, such polymers generally lack sufficient mechanical stability. Yuan et al. [CN 109764980 A, 2019.05.17] used terephthalaldehyde, isophorone diisocyanate, and bis(3-aminopropyl)-terminated poly(dimethylsiloxane) as raw materials for a one-pot reaction to synthesize a silicone elastomer with an elongation at break of 290-1400%, a maximum stress of 165-700 kPa, and a self-healing efficiency of 93.7% at room temperature for 3 hours. Although it exhibits excellent self-healing properties, the elastomer prepared by the one-pot method exhibits poor mechanical stress. In addition, Yuan et al. [CN 110591051 A, 2019.12.20] used terephthalaldehyde, isophorone diisocyanate, bis(3-aminopropyl)-terminated poly(dimethylsiloxane), 3(2-aminoethyl)amine, and 4,4'-diaminodiphenyl disulfide as raw materials to form a triple reversible cross-linked network silicone rubber with 280%, 483kPa, and 5h self-healing efficiency of 94%, and the maximum adhesion strength to iron is 300kPa. However, poor mechanical tensile properties and adhesion properties seriously restrict its further application. Summary of the invention
[0004] In view of the insufficient mechanical tensile and adhesion properties in the prior art, the present invention provides a method for preparing a three-dimensional network structure self-repairing polyurethane with high tensile and strong adhesion properties. The three-dimensional network structure is constructed by a step-by-step reaction method, which greatly enhances the mechanical tensile properties and adhesion strength of the polyurethane.
[0005] The design idea of the present invention is: to address the problem of poor mechanical tensile properties of elastomers, which show low tensile strength and elongation at break, the fundamental problem is the low degree of polymer crosslinking. This patent uses a three-dimensional network structure constructed by a double crosslinking method to enhance mechanical properties. At the same time, the introduction of siloxane bonds and dynamic covalent bonds with oxygen-containing functional groups on the interface can form a dynamic bond that is beneficial to enhancing the interface bonding strength. In addition, the introduction of double dynamic bonds of hydrogen bonds and imine bonds can give it self-healing properties.
[0006] The technical solution of the present invention:
[0007] A method for preparing a three-dimensional network structure self-repairing polyurethane with high tensile strength and strong adhesion performance, using trimesaldehyde as the first cross-linking center and polyether polyol as the second cross-linking point, based on the amide bond formed by the aldehyde group at the 1, 3, 5 positions and the amino group and isophorone diisocyanate to connect the polyether polyol to form a double cross-linked three-dimensional network structure polyurethane with imine bonds and hydrogen bonds; the specific steps are as follows:
[0008] (1) adding trimesic acid aldehyde and bis(3-aminopropyl)-terminated poly(dimethylsiloxane) (NH2-PDMS-NH2) to tetrahydrofuran, and heating and stirring at 60° C. for 2 hours to react to form an oligomer intermediate solution having amino terminal groups;
[0009] (2) After the temperature of the oligomer intermediate solution returns to room temperature, add polyether polyol, stir and dissolve at room temperature, then slowly add tetrahydrofuran solution of isophorone diisocyanate, and finally add dibutyltin dilaurate as a catalyst, heat and stir at 60°C for 4 hours. After the reaction is completed, pour it into a mold, let it stand for 4 hours, and finally bake it in an oven at 40°C for 12 hours to form a three-dimensional network structure polyurethane.
[0010] In the above scheme, the molar ratio of trimesaldehyde to bis(3-aminopropyl)-terminated poly(dimethylsiloxane) (NH2-PDMS-NH2) is 1:3, and the concentration of the tetrahydrofuran solution of bis(3-aminopropyl)-terminated poly(dimethylsiloxane) is controlled within 200 mg / mL for the best effect. The two substances are dissolved in tetrahydrofuran and heated in an oil bath at 60°C, and stirred evenly for 2 hours. The transparent liquid formed is an oligomer intermediate with trimesaldehyde as the center, amino as the terminal group, and connected by amide bonds.
[0011] In the above scheme, the relative molecular mass of the polyether polyol is 2000, the polyether polyol is directly added to the oligomer intermediate solution, and the fluoroquinone diisocyanate is diluted with tetrahydrofuran. The concentration is controlled within 0.5 g / mL for the best effect. The molar ratio of the polyether polyol and the isophorone diisocyanate is 3:6-3:18.
[0012] In the above scheme, the molar ratio of polyether polyol to trimesic acid is 3.6:0.2-3.6:0.4, and the higher the concentration of trimesic acid, the higher the degree of crosslinking. The maximum elongation at break of the obtained polyurethane is 2822.4%, the maximum stress is 26.4MPa, high adhesion strength (5.6MPa for Cu sheet), and self-healing performance (self-healing efficiency is 90.8% at 60°C for 12 hours).
[0013] In the above scheme, dibutyltin dilaurate is used as a catalyst, and the amount is 0.1 mL added to every 10 mL of solution. The mixture is heated in an oil bath at 60° C. and stirred for 4 hours. After the reaction, a viscous transparent liquid is obtained.
[0014] In the above scheme, the viscous transparent liquid is poured into the polytetrafluoroethylene mold while it is hot, and preferably placed in a 0-5°C environment for 4 hours to prevent the solvent from evaporating too quickly and generating bubbles or holes.
[0015] Beneficial effects of the present invention:
[0016] 1) The present invention provides a method for preparing a three-dimensional network structure self-repairing polyurethane with high tensile and strong adhesion properties. Through the design of a double cross-linked three-dimensional network structure, first, an oligomer intermediate with an amino terminal is generated based on trimesaldehyde as the first cross-linking center, and then a polyether polyol is used as the second cross-linking center. The two are connected by isophorone diisocyanate to form a double cross-linked three-dimensional network structure, which enhances the mechanical tensile properties of the elastomer, improves the maximum stress and elongation at break (the maximum elongation at break is 2822.4%, and the maximum stress is 26.4MPa), and the performance is better than the mechanical tensile properties of similar polyurethanes in other literatures. By regulating the content of the double cross-linked structure, the polyurethane has a wide range of tensile stress and strain variations.
[0017] 2) The present invention provides a method for preparing a three-dimensional network structure self-healing polyurethane with high tensile and strong adhesion properties. Two dynamic bonds, imine bonds and hydrogen bonds, are introduced into the system, so that the prepared elastomer can repair itself after damage and has self-healing properties (self-healing efficiency of 90.8% for 12 hours at 60°C), which has application value in the fields of electronic skin and soft robots.
[0018] 3) The present invention provides a method for preparing a three-dimensional mesh structure self-repairing polyurethane with high tensile and strong adhesion performance. The body structure constructed by cross-linking can significantly improve the cohesive strength of the adhesive. The polyurethane prepared under a suitable double cross-linking ratio is transparent and has strong adhesion performance. Different from the polyurethane patch adhesive prepared in the prior art, the polyurethane adhesive exhibits super strong adhesion performance on different materials (5.6MPa for Cu sheet), and has strong cyclic stability, and its performance is significantly better than similar polyurethane patch adhesives in other literature. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The tensile stress-strain curves of polyurethanes with different isophorone diisocyanate contents prepared in Example 2;
[0020] Figure 2 The tensile stress-strain curves of polyurethanes with different oligomer intermediate contents prepared in Example 1;
[0021] Figure 3 This is a stress-strain curve of the PU8 polyurethane prepared in Example 3 without using polyether polyol.
[0022] Figure 4 This is the stress-strain curve of the PU9 polyurethane prepared in Example 4 without using oligomers.
[0023] Figure 5 The bar graph of the adhesion strength of PU2 and PU3 polyurethanes prepared in the present invention to wooden boards;
[0024] Figure 6 A bar graph showing the adhesion strength of the PU2 polyurethane prepared in the present invention to different materials;
[0025] Figure 7 A bar graph showing the adhesion strength of the PU2 polyurethane prepared in the present invention to the wood board at different temperatures;
[0026] Figure 8 A bar graph showing the adhesion strength of the PU2 polyurethane prepared by the present invention to the wood board after five consecutive adhesions at room temperature;
[0027] Fig. 9 These are photos of the PU2 polyurethane prepared by the present invention before and after self-repair and after stretching after repair;
[0028] Fig.10 The original maximum stress of the three polyurethanes PU2, PU6 and PU7 prepared in Example 2 and the maximum stress after repair for 12 hours at different temperatures. DETAILED DESCRIPTION
[0029] The specific implementation of the present invention is further described below in conjunction with the accompanying drawings and technical solutions.
[0030] Example 1
[0031] Step 1: dissolving 0.0324 g:0.96 g, 0.0486 g:1.44 g, and 0.0648 g:1.92 g of trimesaldehyde and bis(3-aminopropyl)-terminated poly(dimethylsiloxane) (NH2-PDMS-NH2) in a molar ratio of 1:3 in 12 mL of tetrahydrofuran (THF), heating and stirring at 60° C. for 2 hours to react and form an oligomer intermediate with an amino terminal group;
[0032] Step 2: First, add 7.2 g of elastomeric polyether polyol to the above three solutions, stir at room temperature to dissolve, then dissolve 2.3976 g of isophorone diisocyanate in 4 mL of tetrahydrofuran solution and slowly add it to the above three solutions, then add 0.1 mL of dibutyltin dilaurate, heat and stir at 60°C for 4 hours, pour into a mold while hot, let stand at 1-5°C for 4 hours, and finally heat in a 40°C oven for 12 hours to obtain PU2, PU6 and PU7 polyurethanes, respectively.
[0033] Example 2
[0034] Step 1: 0.0324 g and 0.96 g of trimesaldehyde and bis(3-aminopropyl)-terminated poly(dimethylsiloxane) (NH2-PDMS-NH2) were dissolved in 12 mL of tetrahydrofuran (THF), respectively, and heated and stirred at 60° C. for 2 hours to react to form an oligomer intermediate with an amino terminal group;
[0035] Step 2: Take the elastomer polyether polyol and isophorone diisocyanate in a molar ratio of 3:6, 3:9, 3:12, and 3:15, and the mass ratios are: 7.2g:2.39g, 7.2g:3.60g, 7.2g:4.80g, 7.2g:6.00g, and 7.2g:7.20g, respectively. First, add the elastomer polyether polyol to the solution of step 1, stir and dissolve at room temperature, then dissolve isophorone diisocyanate in 4mL tetrahydrofuran solution and slowly add it, then add 0.1mL dibutyltin dilaurate, heat and stir at 60°C for 4 hours, pour it into the mold while hot, let it stand at 1-5°C for 4 hours, and finally heat it in a 40°C oven for 12 hours to obtain PU2, PU3, PU4, and PU5 polyurethanes, respectively.
[0036] Example 3
[0037] The difference between the PU2 prepared in Example 3 and Example 2 is that the elastomer polyether polyol is replaced with polyethylene glycol (Mn=2000). The branched polyethylene glycol (Mn=2000) with the same relative molecular mass is selected to better demonstrate the cross-linking point effect of the polyether polyol. The specific steps are as follows:
[0038] Step 1: 0.0324 g and 0.96 g of trimesaldehyde and bis(3-aminopropyl)-terminated poly(dimethylsiloxane) (NH2-PDMS-NH2) were dissolved in 12 mL of tetrahydrofuran (THF), respectively, and heated and stirred at 60° C. for 2 hours to react to form an oligomer intermediate with an amino terminal group;
[0039] Step 2: Take polyethylene glycol (Mn = 2000) and isophorone diisocyanate in a molar ratio of 3:9, with a mass ratio of 7.2g:2.39g. First, add polyethylene glycol (Mn = 2000) to the solution of step 1, stir and dissolve at room temperature, then slowly add isophorone diisocyanate dissolved in 4mL tetrahydrofuran solution, then add 0.1mL dibutyltin dilaurate, heat and stir at 60°C for 4 hours, pour into the mold while hot, let stand at 1-5°C for 4 hours, and finally heat in a 40°C oven for 12 hours to obtain PU8 polyurethane.
[0040] Example 4
[0041] The difference between PU2 prepared in Example 4 and Example 2 is that Example 4 omits the process of preparing the oligomer in step 1, and uses an equal amount of isophorone diisocyanate to replace the oligomer, in order to better demonstrate the cross-linking point effect of preparing the oligomer with trimesaldehyde. The specific steps are as follows:
[0042] First, add the elastomeric polyether polyol (7.2 g) into 12 mL of tetrahydrofuran solution and stir at room temperature to dissolve. Then, dissolve isophorone diisocyanate (2.43 g) in 4 mL of tetrahydrofuran solution and slowly add it to the above solution. Then, add 0.1 mL of dibutyltin dilaurate, heat and stir at 60°C for 4 hours, pour into a mold while hot, let stand at 1-5°C for 4 hours, and finally heat in an oven at 40°C for 12 hours to obtain PU9 polyurethane.
[0043] The mechanical properties of polyurethanes with different isophorone diisocyanate contents in Example 2 were studied using a universal testing machine. The sample used in the tensile test was: 6*0.5*0.2cm 3 The tensile loading rate is 20 mm / min, and the test result is the average of three tests. Figure 1As shown, it is a stress-strain curve of polyurethane with different isophorone diisocyanate contents in Example 2. The elongation at break and the maximum stress of PU2 polyurethane are 2821% and 5.2MPa, respectively; the elongation at break and the maximum stress of PU3 polyurethane are 1984% and 11.1MPa, respectively; the elongation at break and the maximum stress of PU4 polyurethane are 1526% and 15.4MPa, respectively; the elongation at break and the maximum stress of PU5 polyurethane are 1406% and 26.4MPa, respectively. As the content of isophorone diisocyanate increases, the maximum stress gradually increases, while the elongation at break gradually decreases. The elongation at break of PU2 polyurethane reaches a maximum of 2821%, and the maximum stress of PU5 polyurethane reaches a maximum of 26.4MPa.
[0044] like Figure 2 As shown, it is a stress-strain curve of polyurethane with different oligomer intermediate contents in Example 1. The elongation at break and the maximum stress of PU2 polyurethane are 2821% and 5.2MPa respectively; the elongation at break and the maximum stress of PU6 polyurethane are 2236% and 2.75MPa respectively; the elongation at break and the maximum stress of PU7 polyurethane are 1612% and 1.28MPa respectively. As the content of oligomer intermediate increases, the maximum stress gradually decreases, and the elongation at break gradually decreases. The elongation at break of PU2 polyurethane reaches a maximum of 2821%, and the maximum stress of PU2 polyurethane reaches a maximum of 26.4MPa.
[0045] like Figure 3 As shown in the figure, it is a stress-strain curve of PU8 polyurethane prepared in Example 3 without polyether polyol. The elongation at break and the maximum stress of PU8 polyurethane are 85% and 2.46 MPa respectively, which are obviously lower than the mechanical properties of PU3 polyurethane. This is mainly because PU8 polyurethane adopts a linear polyethylene glycol structure, while polyether polyol contains a trihydroxy structure which can be used as a cross-linking center in polyurethane after reaction. Although the oligomer is added as a cross-linking point, the stress can reach 2.46 MPa, but the maximum stress is obviously lower than PU3.
[0046] like Figure 4 As shown in the figure, it is a stress-strain curve of PU9 polyurethane prepared in Example 4 without oligomer. The elongation at break and the maximum stress of PU9 polyurethane are 861% and 0.81MPa respectively, which are obviously lower than the mechanical properties of PU3 polyurethane. PU9 polyurethane has polyether polyol as a crosslinking point, and the elongation at break can reach 861%, but its maximum stress is lower. This is mainly because PU9 polyurethane does not use oligomer as a crosslinking point, and the maximum stress is only 0.81MPa, which is obviously lower than the maximum stress of PU3.
[0047] like Figure 5As shown, it is the adhesion strength bar graph of PU2 and PU3 polyurethanes prepared by the present invention to wooden boards. The adhesion strengths of PU2 and PU3 polyurethanes to wooden boards are 3.21MPa and 0.290MPa respectively. The adhesion strength gap between the two substances to the same substance is relatively large, mainly because the ratio of the amount of polyether polyol to isophorone diisocyanate in PU2 polyurethane is 3:6, and the system still contains excessive polyether polyol, and the excessive hydroxyl can form abundant hydrogen bonding with the substrate to produce strong adhesion. When the ratio of the amount of polyether polyol to isophorone diisocyanate is 3:9, since the hydroxyl groups in the polyether polyol almost all participate in the reaction, low adhesion is shown. And as the ratio increases, the toughness of polyurethane gradually increases, and the hydrogen bonding strength of polyurethane and substrate weakens, thereby causing the adhesion strength to weaken.
[0048] like Figure 6 As shown in the figure, it is a bar graph of the adhesion strength of PU2 polyurethane prepared by the present invention to different materials. The adhesion strength of PU2 polyurethane to PET, PVC, Cu, Fe, glass, Al and wood board are 5.3, 4.1, 5.6, 4.9, 5.5, 4.8 and 3.2 MPa respectively. Among them, the adhesion strength to Cu is the largest at 5.6 MPa, and the adhesion strength to wood board is the smallest at 3.2 MPa.
[0049] like Figure 7 The figure shows the adhesion strength bar graph of the PU2 polyurethane prepared by the present invention at different temperatures. The adhesion strength of the PU2 polyurethane adhered to the wood board at 25°C, 40°C, 60°C and 80°C are 3.2MPa, 3.8MPa, 4.3MPa and 7.3MPa respectively. It shows that with the increase of temperature, the adhesion strength of the polyurethane gradually increases, and the maximum adhesion strength is 7.3MPa at 80°C.
[0050] like Figure 8 As shown in FIG. 1 , it is a bar graph of the adhesion strength of the PU2 polyurethane prepared by the present invention to the wood board for five consecutive times at room temperature. Figure 5 As shown, the strengths of the five consecutive viscosities are 3.7MPa, 3.4MPa, 3.5MPa, 3.4MPa and 2.9MPa respectively. The adhesion strengths of the first five contact adhesions show strong stability.
[0051] like Fig. 9 As shown in the figure, the PU2 polyurethane prepared by the present invention is shown before and after self-repair and stretched after healing. Due to the presence of dynamic bonds such as imine bonds and hydrogen bonds, it can be endowed with outstanding self-repairing properties, and can be repaired and stretched after fracture. Fig.10Shown are the tensile stress-strain curves of the PU2 polyurethane, PU6 and PU7 polyurethanes prepared in Example 1 after original tensile strength and repair at 25°C and 60°C for 12 hours. The maximum stresses of the polyurethanes after self-repairing for 12 hours at 25°C are 1.69MPa, 1.72MPa and 0.85MPa, respectively. The maximum stresses of the polyurethanes after self-repairing for 12 hours at 60°C are 3.5MPa, 2.1MPa and 1.13MPa, respectively. Under the same repair time, as the temperature increases, the maximum stress that the polyurethane can repair becomes larger and larger. PU7 polyurethane can achieve a self-repair efficiency of 90.8% after repairing at 60°C for 12 hours.
[0052] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a three-dimensional network structure self-repairing polyurethane with high tensile and strong adhesion properties, characterized in that: Here are the steps: (1) adding trimesic acid aldehyde and bis(3-aminopropyl)-terminated poly(dimethylsiloxane) to tetrahydrofuran, and heating and stirring at 60° C. for 2 hours to react to form an oligomer intermediate solution having amino terminal groups; (2) After the temperature of the oligomer intermediate solution returns to room temperature, add polyether polyol, stir and dissolve at room temperature, then slowly add tetrahydrofuran solution of isophorone diisocyanate, and finally add dibutyltin dilaurate as a catalyst, heat and stir at 60°C for 4 hours. After the reaction is completed, pour it into a mold, let it stand for 4 hours, and finally bake it in an oven at 40°C for 12 hours to form a three-dimensional network structure polyurethane.
2. The method for preparing a three-dimensional network structure self-repairing polyurethane according to claim 1, characterized in that: The molar ratio of trimesaldehyde to bis(3-aminopropyl)-terminated poly(dimethylsiloxane) is 1:3, and the concentration of the tetrahydrofuran solution of bis(3-aminopropyl)-terminated poly(dimethylsiloxane) is controlled within 200 mg / mL.
3. The method for preparing a three-dimensional network structure self-repairing polyurethane according to claim 1, characterized in that: The relative molecular mass of the polyether polyol is 2000, the concentration of the tetrahydrofuran solution of isophorone diisocyanate is controlled within 0.5 g / mL, and the molar ratio of the polyether polyol to isophorone diisocyanate is 3:6-3:
18.
4. The method for preparing a three-dimensional network structure self-repairing polyurethane according to claim 1, characterized in that: The molar ratio of the polyether polyol to trimesaldehyde is 3.6:0.2-3.6:0.
4.
5. The method for preparing a three-dimensional network structure self-repairing polyurethane according to claim 1, characterized in that: Dibutyltin dilaurate was used as a catalyst, with 0.1 mL added per 10 mL of solution.
6. The method for preparing a three-dimensional network structure self-repairing polyurethane according to claim 1, characterized in that: In step (2), the mold is placed in an environment of 0-5°C and allowed to stand for 4 hours.