Cyclodextrin compound modified polyurethane elastomer and preparation method thereof

By introducing cyclodextrin compounds into polyurethane elastomers and forming intermolecular hydrogen bonds, the problem of insufficient mechanical properties of polyurethane materials is solved, and the mechanical properties and impact resistance of the materials are significantly improved.

CN119060291AActive Publication Date: 2024-12-03BEIJING INST OF TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411185915.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-03
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

The existing polyurethane elastomer materials have shortcomings in terms of mechanical properties and impact resistance, especially the problems of insufficient dispersion of inorganic fillers and poor material stability, resulting in poor mechanical properties.

Method used

The polyurethane elastomer is modified by cyclodextrin compounds, and an intermolecular hydrogen bond is formed between the hard and soft segments of the cyclodextrin and the polyurethane elastomer to enhance the mechanical properties of the material. Specific methods include curing molding using components A and B and cyclodextrin compounds, controlling reaction conditions and component ratios, and ensuring hydrogen bonding and material properties.

Benefits of technology

It effectively improves the mechanical properties and impact resistance of polyurethane materials, enhances the toughness and stability of the materials. Compared with the inorganic filler method, the mechanical properties of cyclodextrin compound modified polyurethane materials have been significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060291A_ABST
    Figure CN119060291A_ABST
Patent Text Reader

Abstract

The invention relates to a cyclodextrin compound modified polyurethane elastomer and a preparation method thereof, and belongs to the technical field of polymers. The cyclodextrin compound modified polyurethane is prepared from the following main raw materials in percentage by mass: a material A and a material B, wherein the material A comprises 44 to 46 percent of diisocyanate substances and 54 to 56 percent of polyalcohol; and the material B comprises the following components in percentage by weight: 70%-74% of polyalcohol, 18%-22% of polyether 330N polyalcohol and 4%-8% of a diol chain extender. Auxiliary raw materials are a cyclodextrin compound, an indicator bromocresol blue and a toluene solution of di-n-butylamine. The cyclodextrin compound modified polyurethane is a novel polyurethane material with excellent mechanical properties, and a cyclodextrin compound in the cyclodextrin compound modified polyurethane can provide a plurality of hydroxyl groups and can form intermolecular hydrogen bonds with macromolecular chain segments, so that the mechanical properties of the polyurethane are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a cyclodextrin compound-modified polyurethane elastomer and a preparation method thereof, belonging to the technical field of elastomer polymers. Background Art

[0002] As an engineering plastic, polyurethane materials have received extensive attention and application in the fields of automobiles, aerospace, special operations, and military. At present, polyurethane elastomer materials with excellent mechanical properties have not been studied much, which also limits the application of polyurethane materials in the field of mechanics. In order to broaden the application scope of polyurethane materials and improve the mechanical and impact resistance of polyurethane, fillers are added to polyurethane materials. Through the full contact between the added fillers and the polyurethane chain segments, physical and chemical changes occur to change the mechanical properties of polyurethane materials and expand their application scope in mechanics.

[0003] Most of the methods for modifying polyurethane elastomers by filler method adopt the method of dispersing and compounding inorganic fillers (such as silica SiO2, carbon nanotubes, etc.). However, inorganic fillers occupy the space for stacking polymer chain segments, which greatly reduces the damping value in the low temperature zone and also leads to insufficient dispersion of inorganic fillers in the polyurethane elastomer matrix. Since the interaction force between inorganic fillers and the polyurethane elastomer matrix is ​​very small, adding more inorganic fillers will lead to easy wear between the polyurethane elastomer matrix and the inorganic fillers, poor material stability, and also cause the polyurethane elastomer to become brittle, that is, the mechanical properties will deteriorate. Summary of the invention

[0004] The technical problem solved by the present invention is: to overcome the shortcomings of the prior art and to propose a polyurethane elastomer modified with a cyclodextrin compound and a preparation method thereof. Since there is a strong hydrogen bond between the cyclodextrin substance and the polar groups inside the polymer, the mechanical properties of the polyurethane material can be enhanced and the toughness can be increased while ensuring its own mechanical properties.

[0005] The technical solution of the present invention is:

[0006] A polyurethane elastomer modified by a cyclodextrin compound, wherein the polyurethane elastomer matrix is ​​modified by using a cyclodextrin compound, the polyurethane elastomer matrix is ​​composed of a hard segment and a soft segment, and intermolecular hydrogen bonds are formed between the cyclodextrin compound and the hard segment and the soft segment of the polyurethane elastomer matrix;

[0007] The structural formula of the polyurethane elastomer modified by the cyclodextrin compound is as follows:

[0008]

[0009] Among them, the dotted line represents the hydrogen bond, and the n value is the number of structural units, which can be obtained by calculating the molecular weight.

[0010] A method for preparing a polyurethane elastomer modified by a cyclodextrin compound, wherein the polyurethane elastomer is obtained by curing and molding a component A, a component B and a cyclodextrin compound, wherein the cyclodextrin compound is a white solid powder, including α-cyclodextrin, β-cyclodextrin or γ-cyclodextrin; the mass of the cyclodextrin compound is 0.5%-5.0% of the mass of the component A and the component B;

[0011] Taking the total mass of raw materials for preparing the A component as 100%, the raw material components and their mass fractions are as follows:

[0012] Diisocyanate 44% to 46%;

[0013] Polyol 54% to 56%;

[0014] Taking the total mass of raw materials for preparing the B component as 100%, the components and their mass fractions of the raw materials are as follows:

[0015] Polyol 70% to 74%;

[0016] Polyether 330N polyol (330N) 18% to 22%;

[0017] Diol chain extender 4% to 8%.

[0018] The diisocyanate is at least one of diphenylmethane diisocyanate (MDI), hexamethylene diisocyanate (HDI), and isophorone diisocyanate (IPDI);

[0019] The polyol is at least one of polytetrahydrofuran (PTMEG) with a molecular weight of 2000 and polytetrahydrofuran (PTMEG) with a molecular weight of 1000;

[0020] The molecular weight of the polyether 330N polyol is 4600-4800;

[0021] The diol chain extender is at least one of 1,4-butanediol (BDO), 1,3-propylene glycol (PDO), ethylene glycol (EG), and 1,5-pentanediol (PTDO).

[0022] A method for preparing a cyclodextrin compound-modified polyurethane elastomer, comprising the steps of:

[0023] (1) Dehydrating the polyol in component A and the polyol, polyether 330N polyol (330N) and diol chain extender in component B, and then mixing the raw materials of component A, diisocyanate and polyol, under the protection of protective gas (stirring during mixing at a stirring speed of 200 r / min), heating to 80-85° C., stirring for reaction for 4-5 hours, and cooling to obtain a viscous polyurethane prepolymer;

[0024] (2) preheating the viscous polyurethane prepolymer obtained in step (1) to 40-50° C., and preheating the polyol, polyether 330N polyol and diol chain extender in component B to 50-70° C. under air-tight conditions;

[0025] (3) stirring the cyclodextrin compound, the viscous polyurethane prepolymer preheated in step (2), the polyol, the polyether 330N polyol and the diol chain extender at a speed of 2000 r / min for 30 to 35 seconds, pouring them into a polytetrafluoroethylene mold, and curing them at 75 to 80° C. for 2 to 4 hours to obtain a cyclodextrin compound-modified polyurethane elastomer;

[0026] In the step (1), the isocyanate content of the obtained polyurethane prepolymer is determined by titration: the polyurethane prepolymer is added to isopropanol, heated and stirred at 45 to 55° C. to dissolve, to obtain a titration sample solution; and then titrated by titration using a toluene solution of bromocresol blue and di-n-butylamine as an indicator to obtain the isocyanate content a in the prepolymer;

[0027] The usage ratio of the polyurethane prepolymer and isopropanol is 3-4 g:500 mL;

[0028] The volume ratio of the titration sample solution to the toluene solution of di-n-butylamine is 2:0.5-1.5; the concentration of the toluene solution of di-n-butylamine is 0.00166 mol / L; the titration reagent used in the titration method is 0.1 mol / L dilute hydrochloric acid;

[0029] The dosage ratio of the bromocresol blue to the titration sample solution is 0.8-1.2 g:1000 mL;

[0030] The R value of the polyurethane prepolymer is controlled at 6.4-6.6;

[0031] The mass relationship of the polyurethane prepolymer, the polyol in component B, the polyether 330N polyol and the diol chain extender satisfies the formula:

[0032] (m1×a%) / 42=R×((m2 / N1)×2+(m3 / N2)×3+(m4 / N3)×2)

[0033] In the formula, m1, m2, m3, and m4 are respectively the masses of the polyurethane prepolymer, the polyol in component B, the polyether 330N polyol, and the diol chain extender; N1, N2, and N3 are respectively the molecular weights of the polyol, the polyether 330N polyol, and the diol chain extender in component B; a is the isocyanate content of the polyurethane prepolymer; the R value is the ratio of the total number of isocyanate groups to the total number of hydroxyl groups, and the R value is 1.04 to 1.06, the total number of isocyanate groups includes the number of isocyanate groups of the diisocyanate in component A, and the total number of hydroxyl groups includes the number of hydroxyl groups of the polyol, the polyether 330N polyol, and the diol chain extender in component B;

[0034] Mix the diisocyanate substance and the polyol, raise the temperature to 80-85°C, and stir for 4-5 hours to obtain a viscous polyurethane prepolymer A material;

[0035] The reacted material A was cooled to room temperature, and isopropanol was added as a solvent to dissolve for 10 minutes in a 50°C water bath, and then the isocyanate content in the prepolymer was obtained by titration;

[0036] Under air-tight conditions, preheat the viscous polyurethane prepolymer to 50°C, and preheat the dehydrated B material polyol, polyether 330N polyol and diol chain extender to 50-70°C;

[0037] The preheated raw materials are stirred at a speed of 2000 r / min for 30 to 35 seconds, poured into a polytetrafluoroethylene mold, and cured at 75 to 80° C. for 2 to 4 hours to obtain a polyurethane elastomer.

[0038] Beneficial Effects

[0039] The invention provides a cyclodextrin compound modified polyurethane elastomer. The polyurethane elastomer consists of two components, A and B. Taking the total mass of the raw materials A and B as 100%, the components and their mass fractions in the raw material A are as follows: 44% to 46% of diisocyanate substances and 54% to 56% of polyols; the components and their mass fractions in the raw material B are as follows: 70% to 74% of polyols, 18% to 22% of polyether 330N polyol (330N), and 4% to 8% of diol chain extenders. The setting of the mass fractions can ensure the balance of -NCO groups and -OH groups in the polyurethane, and simultaneously ensure the deformation ability of the polyurethane while giving it excellent mechanical properties.

[0040] The present invention provides a cyclodextrin compound modified polyurethane elastomer. In the preparation of the polyurethane elastomer, both ends of the diisocyanate substance in the raw material composition of component A contain isocyanate groups, and both ends of the polyol contain hydroxyl groups. After the preliminary synthesis of the prepolymer, the two can be stored for a long time at room temperature. Subsequently, different types of polymer long chain segments (PTMG, PPG, etc.), crosslinking agents (such as 330N, etc.) and chain extenders (such as BDO, PDO, etc.) can be added according to different production needs. The above raw materials can be polymerized at room temperature to produce polyurethane elastomers, and then the cyclodextrin substance is added and dispersed and compounded to obtain the finished product; the method is simple in steps, the experimental formula can be changed according to production needs, and industrial production can be carried out.

[0041] The invention provides a cyclodextrin compound modified polyurethane elastomer. In the preparation of the polyurethane elastomer, the reaction temperature of prepolymer synthesis of 80-85° C. is an important condition for the successful prepolymerization.

[0042] The present invention provides a cyclodextrin compound modified polyurethane elastomer. In the preparation of the polyurethane elastomer, the preheating temperature of the prepolymer needs to be maintained at 40-50°C, which is the key to preserving the prepolymer. The prepolymer will self-polymerize at a temperature of 50-70°C. Both ends of the prepolymer are capped with isocyanate (-NCO) and have a tendency to polymerize with hydroxyl groups in components such as chain extenders and crosslinking agents in the main raw materials at room temperature. This polymerization method can promote the forward reaction and accelerate the reaction rate.

[0043] The present invention provides a cyclodextrin compound modified polyurethane elastomer. In the preparation of the polyurethane elastomer, the isocyanate content of the prepolymer needs to be controlled. Too much isocyanate content will make the polyurethane structure difficult to form and the polyurethane elastomer cannot be obtained; too much hydroxyl group in the main raw material will reduce the mechanical properties of the polyurethane.

[0044] The present invention relates to a cyclodextrin compound modified polyurethane and a preparation method thereof, and belongs to the technical field of polymers. The main raw material composition and mass fraction of the cyclodextrin compound modified polyurethane are as follows: 44% to 46% of diisocyanate substances and 54% to 56% of polyols in material A; 70% to 74% of polyols, 18% to 22% of polyether 330N polyols (330N) and 4% to 8% of diol chain extenders in material B. The auxiliary raw materials are cyclodextrin compounds (α-cyclodextrin, β-cyclodextrin, γ-cyclodextrin, etc.), indicator bromocresol blue and toluene solution of di-n-butylamine. The cyclodextrin compound modified polyurethane is a new type of polyurethane material with excellent mechanical properties. The cyclodextrin compound in the cyclodextrin compound modified polyurethane can provide many hydroxyl groups, can form intermolecular hydrogen bonds with polymer chains, and improve the mechanical properties of polyurethane. The present invention also provides a method for preparing cyclodextrin compound modified polyurethane, wherein the cyclodextrin compound is introduced into the polyurethane system by means of filler dispersion and compounding to generate cyclodextrin compound modified polyurethane material, the method has simple steps, the experimental formula can be changed according to production requirements, and industrial production can be carried out. Moreover, compared with inorganic fillers, organic fillers do not have a fixed rigid structure, can be well dispersed in the polyurethane elastomer matrix, and generate interaction forces with the groups inside the polymer material through their own active groups, forming intermolecular chain segment friction movement, thereby realizing the consumption of external energy and improving the mechanical properties and impact resistance of the composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 The infrared spectra of the polyurethane samples (i.e., Examples 1 to 3) to which β-cyclodextrin is added at mass fractions of 0.5%, 1.0%, and 1.5%;

[0046] Figure 2 The graph is a mechanical property test result diagram of polyurethane samples (i.e., Examples 1 to 3) to which β-cyclodextrin is added at mass fractions of 0.5%, 1.0%, and 1.5%;

[0047] Figure 3 The figure is a result of the dynamic thermomechanical analysis test on the loss factor of the polyurethane samples (ie, Examples 1 to 3) to which β-cyclodextrin is added at mass fractions of 0.5%, 1.0%, and 1.5%. DETAILED DESCRIPTION

[0048] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments, but this is not intended to limit the present invention.

[0049] Example 1

[0050] In this embodiment, the molecular weight of polytetrahydrofuran is 2000, and the molecular weight of polyether 330N polyol is 4600.

[0051] 225 g of diphenylmethane diisocyanate (MDI) and 275 g of polytetrahydrofuran were added to a 500 mL three-necked glass reactor, and the temperature was raised to 80° C. The raw materials were stirred at a rate of 200 r / min to mix them evenly, and a polyurethane prepolymer was obtained after reacting for 4 hours.

[0052] 0.3995 g of the prepolymer obtained in step (1) was dissolved in 50 mL of isopropanol and heated at 50° C. for 10 min to fully dissolve it. 4 drops of bromocresol blue indicator were added and then 25 mL of di-n-butylamine toluene solution was added to completely dissolve the indicator. The isocyanate content in the prepolymer was determined to be 12.86% by titration using 0.1 mol / L dilute hydrochloric acid.

[0053] The ratio of the mass (g) of bromocresol blue to the volume (mL) of the solvent sodium hydroxide in the bromocresol blue indicator is 1:1000, and the concentration of the sodium hydroxide is 0.1 mol / L.

[0054] The prepolymer titrated in step (2) is preheated to 50°C, and the main raw materials after dehydration, polytetrahydrofuran, polyether 330N polyol and 1,4-butanediol are preheated to 70°C.

[0055] Add 0.5% by mass of β-cyclodextrin, 44 g of polytetrahydrofuran in step (3), 10 g of polyether 330N polyol and 3.76 g of 1,4-butanediol to the container in sequence, then add 44.12 g of the prepolymer and stir the solution at a stirring rate of 2000 r / min for 30 s; pour into a polytetrafluoroethylene container and place in an oven at 80° C. for curing for 2 h to obtain a polyurethane elastomer.

[0056] The 0.5% added mass fraction of β-cyclodextrin means that the mass of the added β-cyclodextrin is 0.5% of the total mass of component A and component B;

[0057] The β-cyclodextrin / polyurethane structural formula is as follows: (the dotted lines represent hydrogen bonds)

[0058]

[0059] Example 2

[0060] In this embodiment, the molecular weight of polytetrahydrofuran is 2000, and the molecular weight of polyether 330N polyol is 4750.

[0061] (1) 225 g of diphenylmethane diisocyanate and 275 g of polytetrahydrofuran were added to a 100 mL three-necked flask, and the temperature was raised to 80° C. The raw materials were stirred at a rate of 200 r / min to mix them evenly. After reacting for 4 h, a polyurethane prepolymer was obtained.

[0062] (2) 0.3970 g of the prepolymer obtained in step (1) was dissolved in 50 mL of isopropanol and heated at 50° C. for 10 min to fully dissolve it. 4 drops of bromocresol blue indicator were added and then 25 mL of di-n-butylamine toluene solution was added to completely dissolve the indicator. The isocyanate content in the prepolymer was determined to be 12.97% by titration using 0.1 mol / L dilute hydrochloric acid.

[0063] The ratio of the mass (g) of bromocresol blue in the bromocresol blue indicator to the volume (mL) of the solvent sodium hydroxide is 1:1000, and the concentration of the sodium hydroxide is 0.1 mol / L;

[0064] (3) preheating the prepolymer titrated in step (2) to 50° C., and preheating the main raw materials of dehydrated polytetrahydrofuran, polyether 330N polyol and 1,4-butanediol to 70° C.

[0065] (4) Add 1.0% β-cyclodextrin, 36.61g of polytetrahydrofuran in step (3), 10.37g of polyether 330N polyol and 3.74g of 1,4-butanediol to the container in sequence, and then add 46.55g of prepolymer and stir the solution at a stirring rate of 2000r / min for 30s; pour it into a polytetrafluoroethylene container and put it in an oven at 80°C for curing for 4h to obtain a polyurethane elastomer.

[0066] The added β-cyclodextrin with a mass fraction of 1.0% means that the mass of the added β-cyclodextrin is 1.0% of the total mass of the A component and the B component.

[0067] Example 3

[0068] In this embodiment, the molecular weight of polytetrahydrofuran is 2000, and the molecular weight of polyether 330N polyol is 4800.

[0069] (1) 225 g of diphenylmethane diisocyanate and 275 g of polytetrahydrofuran were added to a 100 mL three-necked flask, and the temperature was raised to 80° C. The raw materials were stirred at a rate of 200 r / min to mix them evenly. After reacting for 4 h, a polyurethane prepolymer was obtained.

[0070] (2) 0.4244 g of the prepolymer obtained in step (1) was dissolved in 50 mL of isopropanol and heated at 50° C. for 10 min to fully dissolve it. 4 drops of bromocresol blue indicator were added and then 25 mL of di-n-butylamine toluene solution was added to completely dissolve the indicator. The isocyanate content in the prepolymer was determined to be 11.55% by titration using 0.1 mol / L dilute hydrochloric acid.

[0071] The ratio of the mass (g) of bromocresol blue to the volume (mL) of the solvent sodium hydroxide in the bromocresol blue indicator is 1:1000, and the concentration of the sodium hydroxide is 0.1 mol / L.

[0072] (3) preheating the prepolymer titrated in step (2) to 50° C., and preheating the main raw materials of dehydrated polytetrahydrofuran, polyether 330N polyol and 1,4-butanediol to 70° C.

[0073] (4) Add 1.5% β-cyclodextrin, 36.01 g of polybutylene glycol in step (3), 9.91 g of polyether 330N polyol and 3.74 g of 1,4-butanediol to the container in sequence, and then add 44.15 g of prepolymer and stir the solution at a stirring rate of 2000 r / min for 30 seconds; pour into a polytetrafluoroethylene container and place in an oven at 80°C for curing for 2 hours to obtain a polyurethane elastomer.

[0074] The 1.5% mass fraction of β-cyclodextrin means that the mass of the added β-cyclodextrin is 1.5% of the total mass of the A component and the B component.

[0075] The final products prepared in Examples 1 to 3 were tested by infrared spectroscopy. Figure 1 As shown, it can be concluded that compared with the polyurethane elastomer matrix, the infrared spectrum of the final product of Example 1 is 3300 cm -1 The peak is broad and blunt, indicating that it is the position of the peak corresponding to the intermolecular hydrogen bond, which further indicates that the cyclodextrin compound forms intermolecular hydrogen bonds with the polyurethane.

[0076] The final products prepared in Examples 1 to 3 were subjected to a tensile test. The test conditions were that a 500N mechanical sensor was used, and the size of the test sample was a small test sample of 4 mm × 50 mm. The test was carried out at a tensile rate of 200 mm / min. The results are as follows: Figure 2 As shown, it can be concluded that the mechanical properties of the polyurethane samples after physical blending of cyclodextrin compounds and heat treatment (the mechanical properties after physical blending treatment with 0.5% mass fraction β-cyclodextrin are about 18MPa, the mechanical properties after treatment with 1.0% mass fraction β-cyclodextrin are about 21MPa, and the mechanical properties after treatment with 1.5% mass fraction β-cyclodextrin are about 19MPa) are 50%, 75% and 58% higher than the mechanical properties of the polyurethane elastomer matrix (about 12MPa), indicating that the polyurethane modified by physical blending of cyclodextrin compounds can be used as a type of polyurethane elastomer, which greatly improves the mechanical properties of polyurethane. The final products prepared in Examples 1 to 3 were subjected to dynamic thermomechanical analysis tests. The conditions of the test samples were controlled at a heating rate of 5K / min, a frequency of 10Hz, and a heating temperature range of -75°C to 100°C. The results are as follows: Figure 3 As shown, it can be seen that the value corresponding to the peak value in Example 2 (i.e., the glass transition temperature Tg) is larger, indicating that its rigidity is stronger and the strength is greater. The internal filler cyclodextrin and the polyurethane system are in full contact and form more hydrogen bonds, thereby improving the mechanical properties of the polyurethane sample.

[0077] In summary, the above are only preferred embodiments of the present invention and are not intended to limit the protection scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A cyclodextrin compound-modified polyurethane elastomer, characterized in that: The structural formula of the polyurethane elastomer modified by the cyclodextrin compound is: The dotted lines represent hydrogen bonds, and the value n is the number of structural units.

2. The polyurethane elastomer modified by a cyclodextrin compound according to claim 1, characterized in that: The cyclodextrin compound is α-cyclodextrin, β-cyclodextrin or γ-cyclodextrin.

3. The polyurethane elastomer modified by a cyclodextrin compound according to claim 1, characterized in that: The raw materials for preparing the polyurethane elastomer include component A, component B and cyclodextrin compound; the mass of the cyclodextrin compound is 0.5%-5.0% of the mass of the component A and the component B; Taking the total mass of raw materials for preparing the A component as 100%, the raw material components and their mass fractions are as follows: Diisocyanate 44% to 46%; Polyol 54% to 56%; Taking the total mass of raw materials for preparing the B component as 100%, the components and their mass fractions of the raw materials are as follows: Polyol 70% to 74%; Polyether 330N polyol 18% to 22%; Diol chain extender 4% to 8%.

4. The polyurethane elastomer modified by a cyclodextrin compound according to claim 1, characterized in that: The diisocyanate is at least one of diphenylmethane diisocyanate, hexamethylene diisocyanate and isophorone diisocyanate; The polyol is at least one of polytetrahydrofuran with a molecular weight of 2000 and polytetrahydrofuran with a molecular weight of 1000; The molecular weight of the polyether 330N polyol is 4600-4800; The diol chain extender is at least one of 1,4-butanediol, 1,3-propylene glycol, ethylene glycol, and 1,5-pentanediol.

5. A method for preparing a polyurethane elastomer modified by a cyclodextrin compound according to any one of claims 1 to 4, characterized in that The steps of the method include: (1) Dehydrating the polyol in component A and the polyol, polyether 330N polyol, and diol chain extender in component B, and then mixing the raw materials of component A, diisocyanate and polyol under protective gas protection, heating to 80-85° C., stirring for reaction for 4-5 hours, and cooling to obtain a viscous polyurethane prepolymer; (2) preheating the viscous polyurethane prepolymer obtained in step (1) to 40-50° C., and preheating the polyol, polyether 330N polyol and diol chain extender in component B to 50-70° C. under air-tight conditions; (3) Mixing the cyclodextrin compound, the viscous polyurethane prepolymer preheated in step (2), the polyol, the polyether 330N polyol and the diol chain extender, and then curing the mixture at 75 to 80° C. for 2 to 4 hours to obtain a polyurethane elastomer modified with the cyclodextrin compound.

6. The method for preparing a cyclodextrin compound-modified polyurethane elastomer according to claim 5, characterized in that: In the step (1), the isocyanate content of the obtained polyurethane prepolymer is determined by titration: the polyurethane prepolymer is added to isopropanol, heated and stirred at 45-55° C. to dissolve, to obtain a titration sample solution; and then titrated by titration using a toluene solution of bromocresol blue and di-n-butylamine as an indicator to obtain the isocyanate content a in the prepolymer.

7. The method for preparing a cyclodextrin compound-modified polyurethane elastomer according to claim 6, characterized in that: The usage ratio of the polyurethane prepolymer and isopropanol is 3-4g:500mL.

8. The method for preparing a cyclodextrin compound-modified polyurethane elastomer according to claim 6, characterized in that: The volume ratio of the titration sample solution to the toluene solution of di-n-butylamine is 2:0.5-1.5; the concentration of the toluene solution of di-n-butylamine is 0.00166 mol / L; and the titration reagent used in the titration method is 0.1 mol / L dilute hydrochloric acid.

9. The method for preparing a cyclodextrin compound-modified polyurethane elastomer according to claim 6, characterized in that: The dosage ratio of the bromocresol blue to the titration sample solution is 0.8-1.2 g:1000 mL; The R value of the polyurethane prepolymer is controlled at 6.4-6.

6.

10. The method for preparing a cyclodextrin compound-modified polyurethane elastomer according to claim 5, characterized in that: The mass relationship of the polyurethane prepolymer, the polyol in component B, the polyether 330N polyol and the diol chain extender satisfies the formula: (m1×a%) / 42=R×((m2 / N1)×2+(m3 / N2)×3+(m4 / N3)×2) In the formula, m1, m2, m3, and m4 are respectively the masses of the polyurethane prepolymer, the polyol, polyether 330N polyol, and the diol chain extender in the B component; N1, N2, and N3 are respectively the molecular weights of the polyol, polyether 330N polyol, and the diol chain extender in the B component; a is the isocyanate content of the polyurethane prepolymer; the R value is the ratio of the total number of isocyanate groups to the total number of hydroxyl groups, and the R value is 1.04 to 1.06, the total number of isocyanate groups includes the number of isocyanate groups of the diisocyanate in the A component, and the total number of hydroxyl groups includes the number of hydroxyl groups of the polyol, polyether 330N polyol, and the diol chain extender in the B component.

Citation Information

Patent Citations

  • Long-lasting antibacterial modified polyurethane and preparation method thereof

    CN109096905A

  • Polyphenolic compound modified polyurethane elastomer and preparation method thereof

    CN116143995A

  • Self-healing and Bacteria Resistant Coating Materials for Various Substrates

    US20180057706A1