Oligomeric sulfosuccinate surfactant and preparation method thereof

The esterification rate and purity of oligosac sulfonate surfactant are improved through specific catalyst preparation methods, and the problems of low esterification rate and purity are solved, and its performance is improved, including emulsification and wetting properties.

CN119060322AInactive Publication Date: 2024-12-03广州市高聚新材料科技有限公司
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411173163.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The low esterification and purity of oligosuccin sulfonate surfactants affect their performance, resulting in reduced hydrophilicity and hydrophobicity, and impurities compete for the interface position, reducing the surfactivity of the active agent.

Method used

Using a specific catalyst preparation method, the esterification rate and purity of the esterified material are improved through the esterification process in steps S1 and S2, including the use of biochar powder, dilute hydrochloric acid solution, sodium humate, ferric chloride hexahydrate, and B Materials such as glycol, sodium acetate, imidazole and sulfuric acid are treated with ultrasonic dispersion, hydrothermal kettle and centrifuge tube to form high-efficiency catalysts to improve the esterification rate.

Benefits of technology

The esterification and purity of the oligosac sulfonate surfactant is significantly improved, thereby improving its performance, including enhanced emulsification, wetting and hard water resistance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an oligomeric sulfosuccinate surfactant and a preparation method thereof, and belongs to the technical field of surfactants. The preparation method of the surfactant comprises the following steps: mixing fatty alcohol-polyoxyethylene ether AEO-7, maleic anhydride and a catalyst, heating and stirring, heating to 80 DEG C, condensing, refluxing and stirring, filtering, and taking a liquid phase to obtain an esterified material; and mixing the esterified material, a sodium sulfite aqueous solution and cetyltrimethylammonium bromide, heating, refluxing, stirring, carrying out suction filtration, and taking a solid phase to obtain the surfactant. By preparing the catalyst in the esterification process, the esterification rate of the esterified material is improved, so that the purity of the esterified material is improved, and the performance of the prepared surfactant is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of surfactants, and in particular relates to an oligomeric succinate sulfonate surfactant and a preparation method thereof. Background Art

[0002] Gemini surfactant molecules contain two or more hydrophilic groups and hydrophobic groups, which are chemically connected to form a surfactant by an intermediate connecting group (Spacer). Compared with traditional surfactants, Gemini surfactants usually have the following characteristics: Gemini surfactants are more likely to aggregate into micelles, that is, they have a relatively low CMC value and are more suitable for use as emulsifiers and dispersants. This is mainly due to the fact that the two ionic head groups connected by chemical bonds in the molecule are tightly connected, so that the hydrophobic groups have a strong interaction, which inhibits the separation caused by electrostatic repulsion between the hydrophilic ionic head groups and enhances the binding between the hydrophobic groups. Gemini surfactants are more likely to be adsorbed and arranged closely on the air / liquid interface, which can effectively reduce surface tension and are usually excellent wetting agents. Oligomeric succinate surfactants have excellent emulsification, wettability, permeability and hard water resistance, good low irritation, low toxicity and other characteristics, and their preparation process is simple, there is no three wastes, and the biodegradability is good, thus becoming an important component of Gemini surfactants. However, the esterification rate and purity of oligosuccinate sulfonate surfactants are key factors affecting their performance. A low esterification rate will reduce the ratio of its hydrophilic and hydrophobic parts, thereby reducing its surface activity and resulting in lower purity. The presence of impurities will compete with surfactant molecules for interfacial positions, reduce the surface activity of the surfactant, and affect product performance. Summary of the invention

[0003] The object of the present invention is to provide an oligomeric succinate sulfonate surfactant and a preparation method thereof, which are used to improve the esterification rate of the oligomeric succinate sulfonate surfactant and increase its purity, thereby improving the performance of the oligomeric succinate sulfonate surfactant.

[0004] The purpose of the present invention can be achieved through the following technical solutions:

[0005] A method for preparing an oligomeric succinate sulfonate surfactant, the method comprising the following steps:

[0006] S1, take fatty alcohol polyoxyethylene ether AEO-7 (purchased from Shanghai Fuqi Industry and Trade Co., Ltd.), maleic anhydride, and catalyst, mix, stir at 60 ° C for 20-30 min, heat to 80 ° C, condense reflux and stir for 2-3 h, filter, and take the liquid phase to obtain esterification material;

[0007] S2. Take the esterification material, sodium sulfite aqueous solution and cetyltrimethylammonium bromide, mix them, reflux and stir at 80-90° C. for 1.5-2.5 hours, filter and take the solid phase to obtain the surfactant.

[0008] As a preferred technical solution of the present invention, in step S1, the mass ratio of the fatty alcohol polyoxyethylene ether AEO-7, maleic anhydride, and catalyst is 1:1.05-1.2:0.06-0.08.

[0009] As a preferred technical solution of the present invention, in step S2, the dosage ratio of the esterification material, the sodium sulfite aqueous solution, and hexadecyltrimethylammonium bromide is 8.8-8.9 g:8.2-8.4 mL:0.12 g; and the mass fraction of sodium sulfite in the sodium sulfite aqueous solution is 40%.

[0010] As a preferred technical solution of the present invention, the preparation of the catalyst comprises the following steps:

[0011] A1. Mix peanut shells, wheat straw and corn straw in a mass ratio of 3-4:0.8-1:0.4-0.6, crush them, and pass through a 100-120 mesh sieve to obtain a mixed powder. Spread the mixed powder in a crucible, then wrap the crucible with tin foil and place it in a muffle furnace. Firing at 400-500° C. for 3-4 hours, cooling, grinding, and passing through a 100-120 mesh sieve to obtain biochar powder.

[0012] A2, soak the biochar powder in a dilute hydrochloric acid solution with a concentration of 0.5 mol / L for 12-18 hours, filter, wash the solid phase with water, vacuum dry at 75°C for 20 hours, cool, and mix with sodium humate to obtain material A;

[0013] A3, take ferric chloride hexahydrate, ethylene glycol, and material A, mix, ultrasonically disperse for 20-30 minutes, add sodium acetate, stir at 50-60 ° C for 1-2 hours, transfer to a hydrothermal kettle, keep warm at 150-180 ° C for 10-12 hours, cool, transfer to a centrifuge tube, perform solid-liquid separation under external magnetic field conditions, wash the solid phase, and vacuum dry at 60 ° C for 6-8 hours to obtain material B;

[0014] A4, take triethylamine hydrochloride, anhydrous aluminum chloride, and n-heptane, mix them, stir them at 70-80°C for 3-4h, and remove n-heptane by rotary evaporation to obtain material C;

[0015] A5. Mix imidazole and 98% concentrated sulfuric acid in an ice-water bath, stir for 20-30 min, add 1-nitropyrazole, and then stir in an oil bath at 55-65°C for 4-6 h, cool, pour the hot liquid into a container filled with ice and stir for 20-30 min, filter, and dry the solid phase in vacuum at 100°C for 8-10 h to obtain material D;

[0016] A6. Mix 2-acrylamide-2-methylpropanesulfonic acid, acrylamide and deionized water, and disperse them ultrasonically for 20-30 min. Add the material C and material D, and stir for 20-30 min. Add ammonium persulfate and methylenebisacrylamide, and stir at 60-70° C. for 1-2 h. Add the material B and soak for 20-30 h. Filter, wash the solid phase, dry it in vacuum at 50° C. for 10-12 h, and crush to obtain the catalyst.

[0017] As a preferred technical solution of the present invention, in step A2, the dosage ratio of the biochar powder, the dilute hydrochloric acid solution, and the sodium humate is 10-20 mg: 200 mL: 1-2 mg.

[0018] As a preferred technical solution of the present invention, in step A3, the dosage ratio of ferric chloride hexahydrate, ethylene glycol, sodium acetate and material A is 3-4 mg: 30-40 mL: 0.6-0.8 mg: 20-30 mg.

[0019] As a preferred technical solution of the present invention, in step A4, the mass ratio of triethylamine hydrochloride, anhydrous aluminum chloride and n-heptane is 3-4:1-2:200.

[0020] As a preferred technical solution of the present invention, in step A5, the dosage ratio of imidazole, 1-nitropyrazole and concentrated sulfuric acid is 0.01-0.012 mol: 0.02-0.025 mol: 8-10 mL.

[0021] As a preferred technical solution of the present invention, in step A6, the mass ratio of material B, 2-acrylamide-2-methylpropane sulfonic acid, acrylamide, deionized water, material C, material D, ammonium persulfate, and methylenebisacrylamide is 10-12: 1-2: 1-2: 50: 0.12-0.14: 0.04-0.06: 0.6-0.8: 0.6-0.8.

[0022] The oligomeric succinate sulfonate surfactant is prepared by the above preparation method.

[0023] Beneficial effects of the present invention:

[0024] The invention discloses an oligomeric succinate sulfonate surfactant and a preparation method thereof. The catalyst in the esterification process is prepared to improve the esterification rate of the esterified material, thereby improving the purity of the esterified material and the performance of the prepared surfactant. DETAILED DESCRIPTION

[0025] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with embodiments.

[0026] Example 1

[0027] A method for preparing an oligomeric succinate sulfonate surfactant comprises the following steps:

[0028] S1, take fatty alcohol polyoxyethylene ether AEO-7, maleic anhydride, and catalyst, mix, stir at 60°C for 20min, heat to 80°C, condense reflux and stir for 2h, filter, take liquid phase to obtain esterification material; the mass ratio of fatty alcohol polyoxyethylene ether AEO-7, maleic anhydride and catalyst is 1:1.05:0.06;

[0029] S2, taking the esterification material, sodium sulfite aqueous solution, and hexadecyltrimethylammonium bromide, mixing them, refluxing and stirring at 80° C. for 1.5 hours, filtering, and taking the solid phase to obtain the surfactant; the amount ratio of the esterification material, sodium sulfite aqueous solution, and hexadecyltrimethylammonium bromide is 8.8g:8.2mL:0.12g; the mass fraction of sodium sulfite in the sodium sulfite aqueous solution is 40%;

[0030] The preparation of the catalyst comprises the following steps:

[0031] A1. Mix peanut shells, wheat straw and corn straw in a mass ratio of 3:0.8:0.4, crush them, and pass them through a 100-mesh sieve to obtain a mixed powder. Spread the mixed powder in a crucible, wrap the crucible with tin foil, place it in a muffle furnace, and sinter it at 400° C. for 3 h. Cool it, grind it, and pass it through a 100-mesh sieve to obtain biochar powder.

[0032] A2, soak the biochar powder in a dilute hydrochloric acid solution with a concentration of 0.5 mol / L for 12 hours, filter, wash the solid phase with water, vacuum dry at 75°C for 20 hours, cool, and mix with sodium humate to obtain material A; the dosage ratio of the biochar powder, dilute hydrochloric acid solution, and sodium humate is 10 mg: 200 mL: 1 mg;

[0033] A3, take ferric chloride hexahydrate, ethylene glycol, and material A, mix them, ultrasonically disperse them for 20 minutes, add sodium acetate, stir them at 50°C for 1 hour, transfer them to a hydrothermal kettle, keep them at 150°C for 10 hours, cool them, transfer them to a centrifuge tube, separate the solid and liquid under external magnetic field conditions, wash the solid phase, and vacuum dry them at 60°C for 6 hours to obtain material B; the dosage ratio of ferric chloride hexahydrate, ethylene glycol, sodium acetate, and material A is 3 mg:30 mL:0.6 mg:20 mg;

[0034] A4, triethylamine hydrochloride, anhydrous aluminum chloride, and n-heptane were mixed, stirred at 70°C for 3h, and n-heptane was removed by rotary evaporation to obtain material C; the mass ratio of triethylamine hydrochloride, anhydrous aluminum chloride, and n-heptane was 3:1:200;

[0035] A5. Mix imidazole and 98% concentrated sulfuric acid in an ice-water bath, stir for 20 min, add 1-nitropyrazole, and then stir in a 55°C oil bath for 4 h, cool, pour the hot liquid phase into a container filled with ice and stir for 20 min, filter, and vacuum dry the solid phase at 100°C for 8 h to obtain material D; the ratio of imidazole, 1-nitropyrazole, and concentrated sulfuric acid is 0.01 mol: 0.02 mol: 8 mL;

[0036] A6. Mix 2-acrylamide-2-methylpropane sulfonic acid, acrylamide and deionized water, ultrasonically disperse for 20 minutes, add the material C and material D, stir for 20 minutes, add ammonium persulfate and methylenebisacrylamide, stir at 60°C for 1 hour, add the material B and soak for 20 hours, filter, wash the solid phase, vacuum dry at 50°C for 10 hours, and crush to obtain the catalyst; the mass ratio of the material B, 2-acrylamide-2-methylpropane sulfonic acid, acrylamide, deionized water, material C, material D, ammonium persulfate and methylenebisacrylamide is 10:1:1:50:0.12:0.04:0.6:0.6.

[0037] Example 2

[0038] A method for preparing an oligomeric succinate sulfonate surfactant comprises the following steps:

[0039] S1, take fatty alcohol polyoxyethylene ether AEO-7, maleic anhydride, and catalyst, mix, stir at 60°C for 25min, heat to 80°C, condense reflux and stir for 2.5h, filter, take liquid phase to obtain esterification material; the mass ratio of fatty alcohol polyoxyethylene ether AEO-7, maleic anhydride, and catalyst is 1:1.12:0.07;

[0040] S2, taking the esterification material, sodium sulfite aqueous solution, and hexadecyltrimethylammonium bromide, mixing them, refluxing and stirring at 85° C. for 2 hours, filtering, and taking the solid phase to obtain the surfactant; the amount ratio of the esterification material, sodium sulfite aqueous solution, and hexadecyltrimethylammonium bromide is 8.85g:8.3mL:0.12g; the mass fraction of sodium sulfite in the sodium sulfite aqueous solution is 40%;

[0041] The preparation of the catalyst comprises the following steps:

[0042] A1. Mix peanut shells, wheat straw and corn straw in a mass ratio of 3.5:0.9:0.5, crush them, and pass them through a 110-mesh sieve to obtain a mixed powder. Spread the mixed powder in a crucible, wrap the crucible with tin foil, place it in a muffle furnace, and sinter it at 450° C. for 3.5 hours. Cool it, grind it, and pass it through a 110-mesh sieve to obtain biochar powder.

[0043] A2. Soak the biochar powder in a dilute hydrochloric acid solution with a concentration of 0.5 mol / L for 15 h, filter, wash the solid phase with water, dry it in a vacuum at 75°C for 20 h, cool it, and mix it with sodium humate to obtain material A; the ratio of the biochar powder, dilute hydrochloric acid solution, and sodium humate is 15 mg: 200 mL: 1.5 mg;

[0044] A3, take ferric chloride hexahydrate, ethylene glycol, and material A, mix them, ultrasonically disperse them for 25 minutes, add sodium acetate, stir them at 55°C for 1.5 hours, transfer them to a hydrothermal kettle, keep them at 165°C for 11 hours, cool them, transfer them to a centrifuge tube, separate the solid and liquid under external magnetic field conditions, wash the solid phase, and vacuum dry them at 60°C for 7 hours to obtain material B; the dosage ratio of ferric chloride hexahydrate, ethylene glycol, sodium acetate, and material A is 3.5 mg: 35 mL: 0.7 mg: 25 mg;

[0045] A4, triethylamine hydrochloride, anhydrous aluminum chloride, and n-heptane were mixed, stirred at 75°C for 3.5h, and n-heptane was removed by rotary evaporation to obtain material C; the mass ratio of triethylamine hydrochloride, anhydrous aluminum chloride, and n-heptane was 3.5:1.5:200;

[0046] A5. Mix imidazole and 98% concentrated sulfuric acid in an ice-water bath, stir for 25 min, add 1-nitropyrazole, and then stir in a 60°C oil bath for 5 h, cool, pour the hot liquid phase into a container filled with ice and stir for 25 min, filter, and vacuum dry the solid phase at 100°C for 9 h to obtain material D; the ratio of imidazole, 1-nitropyrazole, and concentrated sulfuric acid is 0.011 mol: 0.023 mol: 9 mL;

[0047] A6. Mix 2-acrylamide-2-methylpropane sulfonic acid, acrylamide and deionized water, ultrasonically disperse for 25 minutes, add the material C and material D, stir for 25 minutes, add ammonium persulfate and methylenebisacrylamide, stir at 65°C for 1.5 hours, add the material B and soak for 25 hours, filter, wash the solid phase, vacuum dry at 50°C for 11 hours, and crush to obtain the catalyst; the mass ratio of the material B, 2-acrylamide-2-methylpropane sulfonic acid, acrylamide, deionized water, material C, material D, ammonium persulfate and methylenebisacrylamide is 11:1.5:1.5:50:0.13:0.05:0.7:0.7.

[0048] Example 3

[0049] A method for preparing an oligomeric succinate sulfonate surfactant comprises the following steps:

[0050] S1, take fatty alcohol polyoxyethylene ether AEO-7, maleic anhydride, and catalyst, mix, stir at 60°C for 30min, heat to 80°C, condense reflux and stir for 3h, filter, take liquid phase to obtain esterification material; the mass ratio of fatty alcohol polyoxyethylene ether AEO-7, maleic anhydride and catalyst is 1:1.2:0.08;

[0051] S2, taking the esterification material, sodium sulfite aqueous solution, and hexadecyltrimethylammonium bromide, mixing them, refluxing and stirring at 90° C. for 2.5 hours, filtering, and taking the solid phase to obtain the surfactant; the amount ratio of the esterification material, sodium sulfite aqueous solution, and hexadecyltrimethylammonium bromide is 8.9g:8.4mL:0.12g; the mass fraction of sodium sulfite in the sodium sulfite aqueous solution is 40%;

[0052] The preparation of the catalyst comprises the following steps:

[0053] A1. Mix peanut shells, wheat straw and corn straw in a mass ratio of 4:1:0.6, crush them, and pass them through a 120-mesh sieve to obtain a mixed powder. Spread the mixed powder in a crucible, wrap the crucible with tin foil, place it in a muffle furnace, sinter it at 500° C. for 4 h, cool it, grind it, and pass it through a 120-mesh sieve to obtain biochar powder.

[0054] A2, soak the biochar powder in a dilute hydrochloric acid solution with a concentration of 0.5 mol / L for 18 hours, filter, wash the solid phase with water, vacuum dry at 75°C for 20 hours, cool, and mix with sodium humate to obtain material A; the dosage ratio of the biochar powder, dilute hydrochloric acid solution, and sodium humate is 20 mg: 200 mL: 2 mg;

[0055] A3, take ferric chloride hexahydrate, ethylene glycol, and material A, mix them, ultrasonically disperse them for 30 minutes, add sodium acetate, stir them at 60°C for 2 hours, transfer them to a hydrothermal kettle, keep them at 180°C for 12 hours, cool them, transfer them to a centrifuge tube, separate the solid and liquid under external magnetic field conditions, wash the solid phase, and vacuum dry them at 60°C for 8 hours to obtain material B; the dosage ratio of ferric chloride hexahydrate, ethylene glycol, sodium acetate, and material A is 4 mg:40 mL:0.8 mg:30 mg;

[0056] A4, triethylamine hydrochloride, anhydrous aluminum chloride, and n-heptane were mixed, stirred at 80°C for 4 hours, and n-heptane was removed by rotary evaporation to obtain material C; the mass ratio of triethylamine hydrochloride, anhydrous aluminum chloride, and n-heptane was 4:2:200;

[0057] A5. Mix imidazole and 98% concentrated sulfuric acid in an ice-water bath, stir for 30 min, add 1-nitropyrazole, and then stir in a 65°C oil bath for 6 h, cool, pour the hot liquid phase into a container filled with ice and stir for 30 min, filter, and vacuum dry the solid phase at 100°C for 10 h to obtain material D; the dosage ratio of imidazole, 1-nitropyrazole, and concentrated sulfuric acid is 0.012 mol:0.025 mol:10 mL;

[0058] A6. Mix 2-acrylamide-2-methylpropane sulfonic acid, acrylamide and deionized water, ultrasonically disperse for 30 minutes, add the material C and material D, stir for 30 minutes, add ammonium persulfate and methylenebisacrylamide, stir at 70°C for 2 hours, add the material B and soak for 30 hours, filter, wash the solid phase, vacuum dry at 50°C for 12 hours, and crush to obtain the catalyst; the mass ratio of the material B, 2-acrylamide-2-methylpropane sulfonic acid, acrylamide, deionized water, material C, material D, ammonium persulfate and methylenebisacrylamide is 12:2:2:50:0.14:0.06:0.8:0.8.

[0059] Comparative Example 1

[0060] The difference from Example 1 is that no catalyst is added during the reaction process in step S1.

[0061] Comparative Example 2

[0062] The difference from Example 1 is that sodium humate is not added in step A2 during the preparation of the catalyst.

[0063] Comparative Example 3

[0064] The difference from Example 1 is that the preparation of the catalyst comprises the following steps:

[0065] A1. Mix peanut shells, wheat straw and corn straw in a mass ratio of 3:0.8:0.4, crush them, and pass them through a 100-mesh sieve to obtain a mixed powder. Spread the mixed powder in a crucible, wrap the crucible with tin foil, place it in a muffle furnace, and sinter it at 400° C. for 3 h. Cool it, grind it, and pass it through a 100-mesh sieve to obtain biochar powder.

[0066] A2, soak the biochar powder in a dilute hydrochloric acid solution with a concentration of 0.5 mol / L for 12 hours, filter, wash the solid phase with water, vacuum dry at 75°C for 20 hours, cool, and mix with sodium humate to obtain material A; the dosage ratio of the biochar powder, dilute hydrochloric acid solution, and sodium humate is 10 mg: 200 mL: 1 mg;

[0067] A3, triethylamine hydrochloride, anhydrous aluminum chloride, and n-heptane were mixed, stirred at 70°C for 3h, and n-heptane was removed by rotary evaporation to obtain material C; the mass ratio of triethylamine hydrochloride, anhydrous aluminum chloride, and n-heptane was 3:1:200;

[0068] A4. Mix imidazole and 98% concentrated sulfuric acid in an ice-water bath, stir for 20 min, add 1-nitropyrazole, and then stir in a 55°C oil bath for 4 h, cool, pour the hot liquid phase into a container filled with ice and stir for 20 min, filter, and vacuum dry the solid phase at 100°C for 8 h to obtain material D; the ratio of imidazole, 1-nitropyrazole, and concentrated sulfuric acid is 0.01 mol: 0.02 mol: 8 mL;

[0069] A5. Mix 2-acrylamide-2-methylpropane sulfonic acid, acrylamide and deionized water, ultrasonically disperse for 20 minutes, add the material C and material D, stir for 20 minutes, add ammonium persulfate and methylenebisacrylamide, stir at 60°C for 1 hour, add the material A and soak for 20 hours, filter, wash the solid phase, vacuum dry at 50°C for 10 hours, and crush to obtain the catalyst; the mass ratio of the material B, 2-acrylamide-2-methylpropane sulfonic acid, acrylamide, deionized water, material C, material D, ammonium persulfate and methylenebisacrylamide is 10:1:1:50:0.12:0.04:0.6:0.6.

[0070] Comparative Example 4

[0071] The difference from Example 1 is that in the preparation process of the catalyst, the mass ratio of material B, 2-acrylamide-2-methylpropanesulfonic acid, acrylamide, deionized water, material C, material D, ammonium persulfate, and methylenebisacrylamide in step A6 is 10:1:1:50:0.16:0:0.6:0.6.

[0072] Comparative Example 5

[0073] The difference from Example 1 is that in the preparation process of the catalyst, the mass ratio of material B, 2-acrylamide-2-methylpropanesulfonic acid, acrylamide, deionized water, material C, material D, ammonium persulfate, and methylenebisacrylamide in step A6 is 10:1:1:50:0:0.16:0.6:0.6.

[0074] Performance Testing

[0075] Test Example 1

[0076] The esterification rates of the esterified materials obtained in Examples 1-3 and Comparative Examples 1-5 were tested, and the test results are shown in Table 1 below.

[0077] Table 1

[0078] Esterification rate (%) Example 1 99.76 Example 2 99.82 Example 3 99.79 Comparative Example 1 92.78 Comparative Example 2 98.14 Comparative Example 3 97.78 Comparative Example 4 97.03 Comparative Example 5 96.94

[0079] As can be seen from Table 1, the present application adds a homemade catalyst during the esterification process to improve the esterification rate; in Comparative Example 2, sodium humate is not added, resulting in a decrease in the adsorption amount of the prepared catalyst, resulting in a decrease in the esterification rate; in Comparative Example 3, ferrosoferric oxide is not introduced, resulting in a decrease in the aggregation effect of the prepared catalyst, resulting in a decrease in the esterification rate; in Comparative Examples 4-5, the activation ability of the active component is reduced, resulting in a decrease in the collision velocity of the reactants in the reaction process, resulting in a decrease in the esterification rate.

[0080] Test Example 2

[0081] The surfactants prepared in Examples 1-3 and Comparative Examples 1-5 were tested for detergency according to standard GB / T13174-91; the foaming power was tested according to standard GB / T 13173.6-91; the wetting power was tested by the canvas sedimentation method, the canvas weight was 0.37 g, the fishhook weight was 30 mg, the test solution concentration was 0.15%, and the test temperature was 23°C;

[0082] The test results are shown in Table 2 below.

[0083] Table 2

[0084] Decontamination value R (%) Foam height (mm) Wetting time(s) Example 1 83.78 173 73 Example 2 84.12 177 67 Example 3 83.97 176 71 Comparative Example 1 46.78 103 269 Comparative Example 2 59.14 142 114 Comparative Example 3 55.79 138 149 Comparative Example 4 54.78 125 187 Comparative Example 5 52.36 112 214

[0085] It can be seen from Table 2 that due to the decrease in the esterification rate and purity of the esterified material, the performance of the subsequently prepared surfactant is reduced.

[0086] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A method for preparing an oligomeric succinate sulfonate surfactant, characterized in that: The preparation method of the surfactant comprises the following steps: S1, take fatty alcohol polyoxyethylene ether AEO-7, maleic anhydride, and catalyst, mix, stir at 60°C for 20-30min, heat to 80°C, condense reflux and stir for 2-3h, filter, and take the liquid phase to obtain esterification material; S2. Take the esterification material, sodium sulfite aqueous solution and cetyltrimethylammonium bromide, mix them, reflux and stir at 80-90° C. for 1.5-2.5 hours, filter and take the solid phase to obtain the surfactant.

2. The method for preparing an oligomeric succinate sulfonate surfactant according to claim 1, characterized in that: In step S1, the mass ratio of the fatty alcohol polyoxyethylene ether AEO-7, maleic anhydride and catalyst is 1:1.05-1.2:0.06-0.

08.

3. The method for preparing an oligomeric succinate sulfonate surfactant according to claim 1, characterized in that: In step S2, the dosage ratio of the esterification material, the sodium sulfite aqueous solution, and hexadecyltrimethylammonium bromide is 8.8-8.9 g:8.2-8.4 mL:0.12 g; and the mass fraction of sodium sulfite in the sodium sulfite aqueous solution is 40%.

4. The method for preparing an oligomeric succinate sulfonate surfactant according to claim 1, characterized in that: The preparation of the catalyst comprises the following steps: A1. Mix peanut shells, wheat straw and corn straw in a mass ratio of 3-4:0.8-1:0.4-0.6, crush them, and pass through a 100-120 mesh sieve to obtain a mixed powder. Spread the mixed powder in a crucible, then wrap the crucible with tin foil and place it in a muffle furnace. Firing at 400-500° C. for 3-4 hours, cooling, grinding, and passing through a 100-120 mesh sieve to obtain biochar powder. A2, soak the biochar powder in a 0.5 mol / L dilute hydrochloric acid solution for 12-18 hours, filter, wash the solid phase with water, dry under vacuum at 75° C. for 20 hours, cool, and mix with sodium humate to obtain material A; A3, take ferric chloride hexahydrate, ethylene glycol, and material A, mix, ultrasonically disperse for 20-30 minutes, add sodium acetate, stir at 50-60 ° C for 1-2 hours, transfer to a hydrothermal kettle, keep warm at 150-180 ° C for 10-12 hours, cool, transfer to a centrifuge tube, perform solid-liquid separation under external magnetic field conditions, wash the solid phase, and vacuum dry at 60 ° C for 6-8 hours to obtain material B; A4, take triethylamine hydrochloride, anhydrous aluminum chloride, and n-heptane, mix them, stir them at 70-80°C for 3-4h, and remove n-heptane by rotary evaporation to obtain material C; A5. Mix imidazole and 98% concentrated sulfuric acid in an ice-water bath, stir for 20-30 min, add 1-nitropyrazole, and then stir in an oil bath at 55-65°C for 4-6 h, cool, pour the hot liquid into a container filled with ice and stir for 20-30 min, filter, and dry the solid phase in vacuum at 100°C for 8-10 h to obtain material D; A6. Mix 2-acrylamide-2-methylpropanesulfonic acid, acrylamide and deionized water, and disperse them ultrasonically for 20-30 min. Add the material C and material D, and stir for 20-30 min. Add ammonium persulfate and methylenebisacrylamide, and stir at 60-70° C. for 1-2 h. Add the material B and soak for 20-30 h. Filter, wash the solid phase, dry it in vacuum at 50° C. for 10-12 h, and crush to obtain the catalyst.

5. The method for preparing an oligomeric succinate sulfonate surfactant according to claim 1, characterized in that: In step A2, the dosage ratio of the biochar powder, the dilute hydrochloric acid solution, and the sodium humate is 10-20 mg: 200 mL: 1-2 mg.

6. The method for preparing an oligomeric succinate sulfonate surfactant according to claim 1, characterized in that: In step A3, the dosage ratio of ferric chloride hexahydrate, ethylene glycol, sodium acetate and material A is 3-4 mg: 30-40 mL: 0.6-0.8 mg: 20-30 mg.

7. The method for preparing an oligomeric succinate sulfonate surfactant according to claim 1, characterized in that: In step A4, the mass ratio of triethylamine hydrochloride, anhydrous aluminum chloride and n-heptane is 3-4:1-2:

200.

8. The method for preparing an oligomeric succinate sulfonate surfactant according to claim 1, characterized in that: In step A5, the dosage ratio of imidazole, 1-nitropyrazole and concentrated sulfuric acid is 0.01-0.012 mol: 0.02-0.025 mol: 8-10 mL.

9. The method for preparing an oligomeric succinate sulfonate surfactant according to claim 1, characterized in that: In step A6, the mass ratio of material B, 2-acrylamide-2-methylpropanesulfonic acid, acrylamide, deionized water, material C, material D, ammonium persulfate, and methylenebisacrylamide is 10-12: 1-2: 1-2: 50: 0.12-0.14: 0.04-0.06: 0.6-0.8: 0.6-0.

8.

10. An oligomeric succinate sulfonate surfactant obtained by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for synthesizing fatty alcohol polyoxyethylene ether (n) maleic diester by using ultrasound-microwave radiation technology

    CN104211940A

  • Magnetic organic solid base catalyst as well as preparation method and application thereof

    CN108404977A

  • Preparation method of fatty alcohol sulfosuccinic acid monoester disodium salt

    CN116947711A

  • Surfactant Compositions

    US20170051195A1

  • Gemini polyoxyethylene ether succinate surfactant for oil displacement and preparation method therefor

    WO2022099826A1