Crosslinked terminated polyimide with high residual carbon rate and application thereof

By combining cross-linked end-capped polyimide with guanidine phosphate with high carbon residue, the problem of insufficient flammability and heat resistance of polyurethane materials is solved, and its flame retardant grade and mechanical properties are improved. It is suitable for high-temperature environments Applications under.

CN119060334AActive Publication Date: 2024-12-03CHANGZHOU UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411226905.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-12-03
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

Polyurethane materials have disadvantages such as low oxygen index, flammability and high smoke density, which limits its further application, and the heat resistance of guanidine phosphate is relatively poor, limiting its application range in high temperature environments.

Method used

The cross-linked end-capped polyimide with high carbon residue is used as the carbon-forming agent. By combining with guanidine phosphate, the flame retardant grade and mechanical properties of the polyurethane composite materials are improved, and the polyurethane composites are improved through specific synthetic routes and treatment methods. Thermal stability and mechanical properties of imine.

Benefits of technology

The high flame retardancy and mechanical properties of polyurethane composites have been improved, their performance and processing performance at high temperatures have been improved, and their application potential has been expanded.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060334A_ABST
    Figure CN119060334A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of high polymer materials, and particularly relates to cross-linked end-capped polyimide with a high residual carbon rate and application of the cross-linked end-capped polyimide. The preparation method comprises the following steps: dissolving 1, 4, 5, 8-naphthalene tetracarboxylic anhydride and 4, 4 '-diaminobiphenyl-2, 2-dicarboxylic acid in N-N dimethylacetamide, adding maleic anhydride, and reacting at room temperature in a nitrogen atmosphere to obtain PAA; pAA is uniformly dispensed on a glass plate for gradient heating reaction, and PI is obtained. And dissolving polyurethane and guanidine phosphate in N-N dimethylacetamide, dissolving the prepared PI in the N-N dimethylacetamide to obtain a polyurethane mixed solution, uniformly dispensing the mixed solution on a glass plate, and drying to obtain the polyurethane composite material. The polyimide and the flame retardant GP are compounded for use, so that the flame retardant grade of the thermoplastic polyurethane composite material is improved, and the obtained polyurethane composite material has excellent mechanical properties and heat resistance and has a wide prospect in the field of high-performance application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a cross-linked terminated polyimide with a high residual carbon rate and application thereof. Background Art

[0002] Thermoplastic polyurethane elastomer (TPU) is an important organic polymer material with advantages such as wide hardness range, oil resistance, moisture resistance, wear resistance, insulation, shock absorption, and high strength. It is widely used in wires, cables, furniture, building insulation, aerospace insulation, fire retardant coatings, clothing, etc. However, polyurethane materials have disadvantages such as low oxygen index (about 18), flammability and high smoke density, which limit their further application.

[0003] Polyimide (PI) is a high-performance polymer with excellent thermal stability and can maintain structural integrity at high temperatures. They have excellent high temperature resistance and can withstand stress and thermal expansion in high temperature environments without melting or decomposing easily. In addition, polyimide also has excellent mechanical properties, including high strength and stiffness. They can withstand large forces and stresses, and have excellent structural stability and resistance to deformation. At the same time, they also show good chemical stability and can resist erosion by chemicals, solvents and corrosive substances.

[0004] In order to improve the flame retardancy, heat resistance and thermal stability of TPU, flame retardants are usually added to it. Guanidine phosphate (GP) is a phosphorus-based flame retardant, a halogen-free, non-toxic and environmentally friendly flame retardant that meets modern environmental protection requirements. It can also be used for flame retardant treatment of a variety of materials, including wood, paper products, plastics, etc., and has broad application prospects. In addition, guanidine phosphate can also enhance its mechanical properties by increasing the carbonization rate of the material. The increase in the carbonization rate means that the material can form more carbon layers during the combustion process. This carbon layer can not only isolate oxygen and heat, but also enhance the structural strength of the material to a certain extent, thereby improving its mechanical properties. However, the heat resistance of guanidine phosphate is relatively poor, which may limit its scope of application in high temperature environments. Summary of the invention

[0005] The purpose of the present invention is to provide a cross-linked blocked polyimide with a high residual carbon rate, and use it as a carbonizing agent to prepare a polyurethane composite material with high flame retardancy and high mechanical properties. The blocked polyimide provided by the present invention also has good thermal stability, a high residual carbon rate, can maintain high temperature strength, and can be used as a carbonizing agent.

[0006] The preparation method of the thermally cross-linked capped polyimide with a high carbon residue rate of the present invention has the following synthesis route:

[0007]

[0008] The specific preparation steps are as follows:

[0009] (1) Add the dehydrated NN dimethylacetamide (DMAc) solvent to a three-necked flask equipped with a mechanical stirrer, add the diamine monomer 4,4'-diaminobiphenyl-2,2-dicarboxylic acid (DCB) at one time, add the dianhydride monomer 1,4,5,8-naphthalenetetracarboxylic anhydride (NTDA) after the diamine monomer is completely dissolved, and replace with nitrogen 3 to 5 times to ensure that the air in the device is isolated to prevent the dianhydride monomer from hydrolyzing prematurely. After the addition of the diamine and dianhydride monomers, add the end-capping agent MA, and at the same time add an appropriate amount of DMAc to adjust the solid content of the system to 12%. React at room temperature for 8 to 12 hours to obtain PAA;

[0010] Wherein, the molar ratio of dianhydride, diamine and end-capping agent is 1:1.02:1-2;

[0011] (2) Using the thermal imidization method, the obtained PAA is evenly dropped on a glass plate and placed in a high-temperature oven for a gradient temperature reaction. After the reaction is complete, it is taken out and scraped off the glass plate to obtain PI.

[0012] The temperature gradient of thermal imidization is: first react at 80°C, 100°C, and 130°C for 1 hour each; after the solvent is basically evaporated to the film is dry, then react at 180°C-2h, 230°C-2h, and 300°C-2h.

[0013] The present invention also provides a thermoplastic polyurethane composite material with high mechanical properties. By adding heat-crosslinked end-capped polyimide to TPU to construct a crosslinked structure, not only the flexibility can be improved, but also the mechanical properties can be greatly increased.

[0014] The polyurethane composite material is composed of 100 parts of polyurethane, 5-10 parts of guanidine phosphate and 5 parts of the cross-linked terminated polyimide prepared by the invention in parts by mass.

[0015] The preparation method of the polyurethane composite material is as follows: polyurethane and guanidine phosphate are dissolved in NN dimethylacetamide, and after complete dissolution, triethylamine is added to adjust the pH of the solution to alkaline, and then polyimide is added thereto, and after complete dissolution, the obtained mixed solution is evenly dripped on a glass plate and dried to obtain a TPU composite film with high flame retardancy and high mechanical properties.

[0016] Due to the adoption of the above technical solution, the present invention has the following advantages and beneficial effects:

[0017] The polyimide provided by the present invention has a high residual carbon rate under oxygen and nitrogen as shown in thermogravimetric analysis test, and thus can be used as an excellent carbon-forming agent. By compounding with the flame retardant GP, the flame retardant grade of the TPU composite material can be effectively improved, and the polyimide itself has excellent mechanical properties, high strength and rigidity, and the polyimide after end-capping can obtain better mechanical strength, such as tensile strength and impact strength. In addition, the processing performance of the TPU composite material can also be improved, and it has a wide range of application potentials. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is the thermogravimetric analysis spectrum of the polyimide NTDA-DCB synthesized in Example 1. DETAILED DESCRIPTION

[0019] In order to explain the present invention more clearly, the present invention is further described below in conjunction with embodiments. It should be understood by those skilled in the art that the content specifically described below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.

[0020] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods. The experimental materials, reagents, etc. used in the following experimental examples can be obtained through commercial channels or known experimental methods.

[0021] Example 1

[0022] This embodiment provides a thermally cross-linked terminated polyimide with a high carbon residue rate, which has the following repeating structural units. The polyimide is named NTDA-DCB.

[0023]

[0024] The specific preparation method is as follows:

[0025] (1) Water removal and purification of N-dimethylacetamide (DMAc):

[0026] Put 100ml of DMAc into a 250ml single-necked flask, add a rotor and 0.6g of CaH2, put on a balloon to seal, and stir magnetically at room temperature for 24h to fully react. After stirring, set up a vacuum distillation device. Since the boiling point of DMAc is 163℃, the vacuum distillation temperature is set to 155℃. Separate the front and back fractions, collect the rest and seal them, yield: 80%.

[0027] (2) Preparation of thermally cross-linked terminated polyimide NTDA-DCB:

[0028] The dianhydride monomer 1,4,5,8-naphthalenetetracarboxylic anhydride (NTDA) was pretreated in an oven at 170°C for 12 hours. 38 ml of dehydrated DMAc was added to a three-necked flask equipped with a mechanical stirring device, and 4,4'-diaminobiphenyl-2,2-dicarboxylic acid (DCB) (2.7771 g, 10.2 mmol) was added, and nitrogen was replaced 3 times to ensure that the air in the device was removed, and stirred until completely dissolved. The dianhydride monomer 1,4,5,8-naphthalenetetracarboxylic anhydride (NTDA) (2.6422 g, 10 mmol) was added in four times, half of the total amount was added for the first time, and the amount added each time was half of the previous amount, with an interval of 40 minutes between each batch. After the addition of the dianhydride monomer and the diamine monomer was completed, a capping agent (MA) (1.9612 g, 20 mmol) was added, and DMAc was added to adjust the solid content of the system to 12%, and stirred at room temperature for 8 hours to obtain a PAA acid solution.

[0029] The glass sheet was placed in a high-temperature oven for preheating, and then the PAA acid solution obtained above was drop-coated on the glass sheet for thermal imidization to obtain a PI film with a thickness of 200 μm.

[0030] The temperature gradient of thermal imidization is: first react at 80°C, 100°C, and 130°C for 1 hour each; after the solvent is basically evaporated to the film is dry, then react at 180°C-2h, 230°C-2h, and 300°C-2h. After the reaction is complete, take it out and scrape it from the glass plate to obtain polyimide PI.

[0031] (3) Preparation of TPU composite film:

[0032] Thermoplastic polyurethane (TPU, 3.1578 g) and guanidine phosphate (GP, 0.3158 g) were weighed into a 50 ml beaker, 32.09 mL DMAc was added, and the mixture was placed on a stirring table and heated to 90° C. to stir and dissolve. The mixture was stirred vigorously for 6 h to obtain a 10 wt% TPU solution.

[0033] Triethylamine was added to the TPU solution to adjust the pH value of the solution to 10 to facilitate the dissolution of polyimide, and then polyimide (PI, 0.1579 g) was weighed into the TPU solution and stirred for 8 h. After the solution was completely dissolved, the relevant TPU composite solution was obtained.

[0034] The amount of guanidine phosphate (GP) added is 10 wt % expressed as a weight percentage of the thermoplastic polyurethane (TPU), and the amount of polyimide (PI) added is 5 wt % expressed as a weight percentage of the thermoplastic polyurethane (TPU).

[0035] The TPU composite solution obtained in the above steps was placed in an ultrasonic cleaning machine for 45 minutes, and then allowed to stand for 6 hours to remove bubbles that may be contained in the solution during stirring. After standing completely, it was placed in a vacuum oven to draw a vacuum to completely remove the bubbles contained in the solution. The treated TPU composite solution was then evenly dripped on a glass plate, placed in an oven and dried at 60°C for 10 hours to remove excess moisture, and a related TPU composite film was obtained.

[0036] Example 2

[0037] The difference between this embodiment and embodiment 1 is that the molar ratio of dianhydride, diamine and end-capping agent in the prepared composite film is 1:1.02:1, and other treatment methods are consistent with those in embodiment 1.

[0038] Example 3

[0039] The difference between this embodiment and embodiment 1 is that the ratio of carbon dioxide to carbon dioxide in the prepared composite film is 1:1.02:1.5, and the other processing methods are consistent with those in embodiment 1.

[0040] Example 4

[0041] The difference between this embodiment and embodiment 1 is that the content of flame retardant GP in the prepared composite film is 5 wt %, and other processing methods are consistent with those in embodiment 1.

[0042] Example 5

[0043] The difference between this embodiment and embodiment 1 is that the content of flame retardant GP in the prepared composite film is 7.5wt%, and other processing methods are consistent with those in embodiment 1.

[0044] Comparative Example 1

[0045] The difference between this comparative example and Example 1 is that the thermally cross-linked terminated polyimide is not added to the TPU composite solution, and the other treatment methods are consistent with those in Example 1.

[0046] Comparative Example 2

[0047] The difference between this comparative example and Example 1 is that the dianhydride monomer in the cross-linked terminated polyimide is replaced with hexafluorodianhydride (6FDA) as a carbon-forming agent, and the other treatment methods are consistent with those in Example 1.

[0048] Comparative Example 3

[0049] The difference between this comparative example and Example 1 is that no end-capping agent MA is added to synthesize the thermally cross-linked end-capped polyimide, and other processing methods are consistent with those in Example 1.

[0050] Comparative Example 4

[0051] The difference between this comparative example and Example 1 is that the flame retardant GP is not added, and the other treatment methods are the same as those in Example 1.

[0052] The prepared TPU composite film was subjected to a vertical combustion performance test, and the test results are shown in Table 1

[0053] Table 1

[0054]

[0055] The mechanical properties of the prepared TPU composite film were tested, and the test results are shown in Table 2

[0056] Table 2

[0057] sample Elongation at break / % Tensile strength / MPa Elastic modulus / MPa Example 1 596 36 7.2 Example 2 1053 29 5.3 Example 3 917 34 4.4 Example 4 604 33 6.5 Example 5 653 33 6.9 Comparative Example 1 594 22 3.8 Comparative Example 2 580 25 6.8 Comparative Example 3 517 27 4.9 Comparative Example 4 612 26 5.1

[0058] In summary, the thermally cross-linked terminated polyamide-imide resin prepared in the present application has a high residual carbon rate and can be used as a carbon-forming agent. When used in combination with the flame retardant GP, it can effectively improve the flame retardant grade and mechanical properties of the TPU composite film.

[0059] The above is only a preferred embodiment of the present invention, and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment, it is not used to limit the present invention. Any technician familiar with this patent can make some changes or modify the technical contents suggested above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the solution of the present invention.

Claims

1. A cross-linked terminated polyimide with a high carbon residue rate, characterized in that: The cross-linked terminated polyimide has the following repeating structural units:

2. The cross-linked terminated polyimide with a high residual carbon rate according to claim 1, characterized in that: The preparation method of the cross-linked terminated polyimide has the following steps: (1) dissolving 1,4,5,8-naphthalenetetracarboxylic anhydride NTDA and 4,4'-diaminobiphenyl-2,2-dicarboxylic acid DCB in NN dimethylacetamide, stirring until completely dissolved under a nitrogen atmosphere to obtain a transparent solution; then adding a capping agent MA, and simultaneously adding DMAc to adjust the solid content of the system, stirring and reacting at room temperature to obtain a PAA solution; (2) The obtained PAA solution is evenly dropped onto a glass plate for a gradient temperature reaction. After the reaction is complete, the PAA solution is taken out and scraped off the glass plate to obtain polyimide PI.

3. The cross-linked terminated polyimide with a high carbon residue rate according to claim 2, characterized in that: The molar ratio of 1,4,5,8-naphthalenetetracarboxylic anhydride, 4,4'-diaminobiphenyl-2,2'-dicarboxylic acid and end-capping agent MA in step (1) is 1:1.02:1-2; during the reaction, the solid content of the solution is 12%.

4. The cross-linked terminated polyimide with a high residual carbon rate according to claim 2, characterized in that: The reaction conditions of step (1) are: stirring the reaction at room temperature for 8 to 12 hours.

5. The cross-linked terminated polyimide with a high residual carbon rate according to claim 2, characterized in that: The gradient temperature increase reaction in step (2) is: first react at 80°C, 100°C, and 130°C for 1 hour each; after the solvent evaporates to the film dryness, react at 180°C for 2 hours, 230°C for 2 hours, and 300°C for 2 hours.

6. An application of the cross-linked terminated polyimide with a high carbon residue rate according to claim 1, characterized in that: The cross-linked terminated polyimide with a high residual carbon rate is used as a carbon-forming agent for preparing a polyurethane composite material with high flame retardancy and high mechanical properties.

7. The use of the cross-linked terminated polyimide with a high carbon residue rate according to claim 6, characterized in that: The polyurethane composite material is composed of: 100 parts of polyurethane, 5-10 parts of guanidine phosphate, and 5 parts of the cross-linked terminated polyimide according to claim 1.

8. The use of the cross-linked terminated polyimide with a high carbon residue rate according to claim 6, characterized in that: The preparation method of the polyurethane composite material is as follows: polyurethane and guanidine phosphate are dissolved in NN dimethylacetamide, and after they are completely dissolved, triethylamine is added to adjust the pH of the solution to be alkaline, and then polyimide is added thereto, and after they are completely dissolved, the obtained mixed solution is evenly dripped on a glass plate and dried to obtain a TPU composite film with high flame retardancy and high mechanical properties.

Citation Information

Patent Citations

  • Green water-soluble polyimide high-strength film and preparation method thereof

    CN115948054A

  • Preparation method of high-transparency low-yellowing high-performance polyamide acid resin and polyimide film