Cellulose nanofiber-prolamin composite membrane as well as preparation method and application thereof

By extracting and modifying cellulose and sorghum glycolin from the lees, cellulose nanofiber-sorghum glycolin composite membrane was prepared, which solved the problems of low thermal stability and poor mechanical properties of the protein-based film, and achieved higher Thermal stability and tensile strength are suitable for food packaging and reduce production costs.

CN119060376APending Publication Date: 2024-12-03BEIJING TECH & BUSINESS UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410994193.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the prior art, protein-based films have low thermal stability and poor mechanical properties, which cannot meet the needs of food packaging. Moreover, the study on extracting cellulose and sorghum glycoprotein from wine lees and comprehensive utilization has not been reported, resulting in poor performance of composite membranes. Good and costly.

Method used

Cellulose nanofibers were prepared by extracting cellulose and sorghum glycolin from wine lees and modifying cellulose. The cellulose nanofiber-sorghum glycolin composite membrane was prepared by combining solution casting to improve its thermal stability and Tensile strength.

Benefits of technology

It significantly improves the thermal stability and tensile strength of the composite film, makes up for the disadvantage of protein film formation alone, is suitable for food packaging, and is simple in preparation, easy to obtain raw materials, and low-price.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060376A_ABST
    Figure CN119060376A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of membranes, in particular to a cellulose nanofiber-prolamin composite membrane as well as a preparation method and application thereof. Comprising the following steps: drying and crushing vinasse, and extracting prolamin by adopting an alcohol-alkali method; extracting cellulose through an ultrasonic alkaline method by utilizing the residual precipitate after the alcohol-soluble protein is extracted; cellulose is subjected to TEMPO oxidation and high-pressure homogenization to prepare cellulose nanofibers. Cellulose nanofibers and sorghum prolamin are mixed, and a solution casting method is adopted to prepare the cellulose nanofiber-sorghum prolamin composite membrane. The preparation method is simple, and raw materials are easy to obtain and low in price; through the cross-linking effect of the cellulose nanofibers and the sorghum prolamin, the light transmittance, the thermal stability and the tensile strength of the composite film are remarkably improved, the defect that the protein forms a film independently is overcome, and the composite film is more suitable for food packaging. Meanwhile, the additional value of the vinasse is improved, and technical reference is provided for further research of the composite membrane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of membrane technology, and in particular to a cellulose nanofiber-alcohol-soluble protein composite membrane and a preparation method and application thereof. Background Art

[0002] Bio-based packaging materials have become an emerging trend in food development due to their degradability, non-toxicity and low cost. Protein is a natural biopolymer packaging film matrix. Compared with polysaccharides and lipids, protein-based films have better gas and liquid barrier properties and have attracted extensive attention from researchers. However, with the continuous improvement of food packaging requirements, single-component protein films have disadvantages such as low thermal stability and poor mechanical properties, which cannot meet the needs of packaging materials. In recent years, researchers usually use modified proteins or add modified materials to make up for the shortcomings of poor stability of protein alone. Kafirin has hydrophobicity and self-assembly properties, lacks essential amino acids, and is difficult to be digested by the human body. It can be used to prepare protein-based films, while cellulose nanofibers (CNFs) have the advantages of strong hydrophobicity and high mechanical strength. They can be used as nanomaterial enhancers. Adding cellulose nanofibers as modified materials to kafirin can just make up for the shortcomings of protein alone.

[0003] Wine lees contain high levels of crude fiber, starch, protein, etc. If these components are extracted and utilized, it can not only achieve high-value utilization of wine lees, but also reduce environmental pollution. Cellulose and kafirin are the two chemical components with the highest content in Luzhou-flavor liquor wine lees, but so far, there has been no report on the simultaneous extraction and comprehensive utilization of kafirin and cellulose in wine lees.

[0004] In the prior art, CN117946550A, a nano-network structure chitosan-based edible film, its preparation method and application, CN115232367B, a nano-cellulose-based antibacterial and anti-oxidative hydrophobic film, its preparation method and application, CN117136996A, a coating film for nuts in an aqueous system, its preparation method and application, CN110692712B, a chitosan-zein coating film for preserving chestnuts, and its preparation method, etc., although patent documents also disclose the use of cellulose nanofibers-zein to form a composite film, the main raw material source of the composite film is complex and the cost is high; it is impossible to improve the additional utilization value of wine lees. And the performance of the prepared composite film is not good. Summary of the invention

[0005] The purpose of the present invention is to address the shortcomings of the prior art and provide a method for preparing a cellulose nanofiber-alcohol-soluble protein composite film, by simultaneously extracting cellulose and alcohol-soluble protein from wine lees, and modifying the cellulose to prepare cellulose nanofibers, and then using the cellulose nanofibers and kafirin to prepare a composite film. The thermal stability and tensile strength of the composite film are significantly improved, which makes up for the shortcomings of protein alone in forming a film.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A method for preparing a cellulose nanofiber-prolamin composite film comprises the following steps:

[0008] 1) drying and crushing the wine lees, and extracting alcohol-soluble protein by an alcohol-alkali method; and extracting cellulose by an ultrasonic alkali method using the remaining precipitate after the alcohol-soluble protein is extracted;

[0009] 2) preparing cellulose nanofibers by TEMPO oxidation (2,2,6,6-tetramethylpiperidin-1-oxyl free radical) combined with high pressure homogenization of the cellulose obtained in step 1);

[0010] 3) The cellulose nanofibers prepared in step 2) are mixed with the kafirin prepared in step 1), and a cellulose nanofiber-kafirin composite film is prepared by a solution casting method.

[0011] Preferably, the lees are fresh lees or thawed frozen liquor lees.

[0012] Preferably, the extracted prolamin comprises kafirin.

[0013] Preferably, the powder is screened, degreased and desugared after being crushed.

[0014] Preferably, the cellulose is extracted, bleached with NaClO2, and freeze-dried to obtain cellulose powder.

[0015] Preferably, in the TEMPO oxidation process in step (2), NaClO is the oxidant, and TEMPO and NaBr are the catalysts.

[0016] In the present invention, "white wine lees" refers to the residue left after brewing wine with sorghum and other brewing materials, such as rice and wheat.

[0017] Preferably, in step 1), the mesh size of the sieving is 40 meshes; in the degreasing process, n-hexane is used for degreasing, wherein the ratio of vinasse powder to n-hexane is 1 g:10 mL.

[0018] Preferably, in step 1), the conditions for the sugar removal treatment are: adding xylanase, thermostable α□ amylase and glucanase to the material to enzymatically hydrolyze the polysaccharides in the material, and removing the low molecular weight soluble sugars after enzymatic hydrolysis by centrifugation.

[0019] Preferably, the enzymatic hydrolysis temperature of the xylanase is 50-60°C, the pH is 5.5-6.0, and the enzyme activity is 60U / g;

[0020] The enzymatic hydrolysis temperature of the thermostable α□ amylase is 40-55°C, the pH is 5.5-6.5, and the enzyme activity is 2000U / g;

[0021] The enzymatic hydrolysis temperature of the glucanase is 50-55° C., the pH is 6.0-6.5, and the enzyme activity is 500 U / g.

[0022] Preferably, the centrifugal force used in the centrifugation is 1000-12000 rpm, the centrifugal temperature is 4-25° C., the centrifugal time is 10-15 min, and the supernatant is removed.

[0023] Preferably, in step 1), the ethanol concentration is 65-75%, and the base is NaOH.

[0024] Preferably, in step 1), the concentration of sodium metabisulfite produced by the alcohol-alkali process is 5 g / L, and the concentration of NaOH is 3-3.5 g / L.

[0025] Preferably, the conditions for alkalization by ultrasonic alkali method in step 1) include: reaction time 3-5h, reaction temperature 50-70°C; NaOH mass fraction: 2-4%.

[0026] Preferably, in step 1), the ultrasonic alkali method, the ultrasonic time is 10-30 min.

[0027] Preferably, in step 2), the NaClO oxidation concentration is 25-40 mmol / g, the pH is 9.8-10.2, the high-pressure homogenization pressure is 500-600 bar, and the cycle is repeated 10 times.

[0028] Preferably, in step 3), the concentration of kafirin is 5%-7% (w / v), and the concentration of cellulose nanofibers is 0%-1.5%.

[0029] The present invention also provides a cellulose nanofiber-alcohol-soluble protein composite membrane, which is prepared by the above preparation method.

[0030] Preferably, when the addition amount of cellulose nanofibers is 1%, the thickness of the cellulose nanofiber-kafirin composite film is 47.6 μm, which is less thick and has a smoother surface than the protein film.

[0031] Preferably, when the addition amount of cellulose nanofibers is 1%, the maximum tensile strength of the cellulose nanofiber-kafirin composite film is 9.17 MPa, which is 104% higher than the tensile strength of the protein film.

[0032] Preferably, when the addition amount of cellulose nanofibers is 1%, the decomposition temperature of the cellulose nanofiber-kafirin composite film is 225° C., the decomposition temperature of the protein film is 241° C., and the composite film exhibits better thermal stability.

[0033] The present invention also provides an application of a cellulose nanofiber-prolamin composite film in green food packaging, which is prepared by the above-mentioned preparation method.

[0034] Preferably, when the addition amount of cellulose nanofibers is 1%, the thickness of the cellulose nanofiber-kafirin composite film is 47.6 μm, which is less thick and has a smoother surface than the protein film.

[0035] Preferably, when the addition amount of cellulose nanofibers is 1%, the maximum tensile strength of the cellulose nanofiber-kafirin composite film is 9.17 MPa, which is 104% higher than the tensile strength of the protein film.

[0036] Preferably, when the addition amount of cellulose nanofibers is 1%, the decomposition temperature of the cellulose nanofiber-kafirin composite film is 225° C., the decomposition temperature of the protein film is 241° C., and the composite film exhibits better thermal stability.

[0037] The beneficial effects of the present invention are as follows:

[0038] The preparation method of the invention is simple, the raw materials are easily available and the price is low; the invention provides a method for simultaneously extracting cellulose and kafirin from liquor lees, and preparing a composite film using cellulose nanofibers and kafirin. The cellulose nanofiber-kafirin composite film prepared by the invention significantly improves the tensile strength and thermal stability of the protein film, can make up for the disadvantages of single protein component film formation, and is more suitable for food packaging. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 This is the infrared spectrum of cellulose and CNF25 in Example 1;

[0040] Figure 2 is the XRD pattern of cellulose and CNF25 in Example 1;

[0041] FIG3 is a macroscopic morphology and particle size diagram of CNF25 of Example 1 and CNF10 of Comparative Example 1;

[0042] Figure 4 The infrared spectra of the composite film of Example 1 and the composite film of Comparative Example 2 are shown;

[0043] Figure 5 The surface morphology and cross-sectional view of the composite membrane of Example 1 and the composite membranes of Comparative Examples 2 and 3;

[0044] Figure 6 Thermogravimetric analysis diagrams of the composite membrane of Example 1 and the composite membrane of Comparative Example 2;

[0045] Figure 7 The light transmittance graph of the composite film of Example 1 and the composite films of Comparative Examples 2 and 3;

[0046] Figure 8 The mechanical properties diagram of the composite membrane of Example 1 and the composite membranes of Comparative Examples 2 and 3 are shown. DETAILED DESCRIPTION

[0047] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments and drawings. It should be understood by those skilled in the art that the content described below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.

[0048] Example 1

[0049] A method for preparing a liquor lees cellulose nanofiber-kafirin composite film is prepared by the following steps:

[0050] S1: Extraction of kaorilin and cellulose from liquor lees.

[0051] 1) Pre-treatment

[0052] First, thaw the frozen lees, wash with water until neutral, and dry at 45°C. Use a universal grinder to grind the lees and pass through a 40-mesh sieve.

[0053] 2) Fat removal

[0054] Weigh 50g of dried vinasse powder, add n-hexane at a solid-liquid ratio of 1:10 (m:L), stir mechanically in a 50℃ water bath for 30min, filter, pour off the filtrate, and retain the solid. Repeat the degreasing 3 times, and place in a fume hood to dry for later use.

[0055] 3) Sugar removal

[0056] Add deionized water to the vinasse powder obtained in step 2) at a solid-liquid ratio of 1:10. Then add thermostable α-amylase, xylanase and amyloglucosidase to the vinasse aqueous solution in an amount of 0.5% of the weight of the vinasse powder. The temperature is set to 45°C, the enzymolysis time is 24h, and the pH is 6.5. After enzymolysis, centrifuge at 8000rpm at 4°C for 15min to remove the supernatant to obtain desugared vinasse powder.

[0057] 4) Extraction of kafirin

[0058] A 70% ethanol aqueous solution was used as the extractant, 5 g / L sodium metabisulfite and 3.5 g / L NaOH were added at a solid-liquid ratio of 1:10, the mixture was stirred and extracted at 70°C for 1 h, centrifuged at 6000 rpm for 10 min at 25°C, the extraction was repeated 3 times, and the supernatant was collected; the supernatant was diluted to 40% ethanol by volume and placed in a -20°C refrigerator for 12 h; centrifuged at 8000 rpm at 25°C for 10 min, the precipitate was collected, and the precipitate was washed 3 times with deionized water, and lyophilized to obtain sorghum alcohol-soluble protein powder.

[0059] 5) Remove residual protein (sorghum glutenin, globulin, albumin)

[0060] The precipitate obtained by centrifugation in the first step of step 4) was dried in an oven at 50°C, and the obtained vinasse powder was added with deionized water at a ratio of 1:10, and alkaline protease was added, the enzyme dosage was 0.5% of the mass of the original vinasse powder, and the enzymatic hydrolysis was carried out at 45°C for 12h, and the pH was 10. After enzymatic hydrolysis, the supernatant was removed by centrifugation at 12000rpm at 25°C for 15min to obtain vinasse powder without residual protein.

[0061] 6) Alkaline hydrolysis

[0062] The protein-removed vinasse powder in step 5) is added with deionized water at a solid-liquid ratio of 1:10, and 3% by mass of NaOH is added, and alkaline hydrolysis is performed at 60° C. for 4 hours, and ultrasonic-assisted extraction is performed for 20 minutes. The supernatant is removed by centrifugation and the precipitate is collected.

[0063] 7) Bleaching, removing lignin, hemicellulose and pectin

[0064] Add 3% sodium chlorite solution to the above precipitate, adjust the pH to 3.5, and heat at 75°C for 2h. Sodium chlorite can oxidatively remove lignin, and under acidic conditions, it can remove the remaining pectin, hemicellulose and other substances, so that the purity of cellulose is further improved. Finally, wash with water until neutral, centrifuge at 10000rpm at 25°C for 10min, retain the precipitate, and freeze-dry to obtain cellulose powder.

[0065] S2: Preparation of cellulose nanofibers. Accurately weigh 0.016g TEMPO (0.1mmol) and 0.1g NaBr (1mmol) and dissolve in 100mL deionized water, add 0.5g dry cellulose sample, stir well, and adjust the pH to 10. Add 25mmol / g NaClO solution for oxidation, stir evenly at 500rpm with a magnetic stirrer at room temperature, and continuously add 0.5mol / L NaOH during the oxidation process to maintain the pH of the reaction system between (10±0.2). When the pH is stable and no longer changes (about 3-4h), add 10mL ethanol to terminate the reaction, and adjust the pH to neutral with 0.5mol / L HCl. The lower precipitate was removed by centrifugation (1000 rpm, 10 min) and rinsed three times with ethanol (95% by volume) and deionized water to remove excess salt and impurities. The precipitate was then dispersed in 200 mL of deionized water again and homogenized 10 times in a high-pressure homogenizer at a pressure of 500 bar. The obtained nanocellulose solution was freeze-dried to obtain cellulose nanofibers.

[0066] S3: Preparation of cellulose nanofiber-kafirin composite film. 6% (w / v) kafirin and 2.5% (v / v) polyethylene glycol (PEG-300) were dissolved in 70% ethanol aqueous solution and stirred at 70°C for 1 h under a magnetic stirrer. 1% cellulose nanofibers were added to the solution and continued to stir at 70°C for 1 h. The mixture was homogenized at 12000 rpm for 10 min and ultrasonicated for 10 min. The cellulose nanofiber-kafirin mixture was cast on a mold using a solution casting method and kept in an oven at 60°C for 8 h. The dried and formed film was removed from the oven and cooled at room temperature, and the cast film was gently lifted from the mold to obtain a cellulose nanofiber-kafirin composite film.

[0067] Example 2

[0068] In step 6 of S1), deionized water is added at a material-liquid ratio of 1:10, and 2% by mass of NaOH is added, and the alkaline hydrolysis is carried out at 60° C. for 5 h, and ultrasonic-assisted extraction is performed for 20 min, the supernatant is removed by centrifugation, and the precipitate is collected. The other steps are the same as those in S1 of Example 1.

[0069] Accurately weigh 0.016g TEMPO (0.1mmol) and 0.1g NaBr (1mmol) in S2 and dissolve in 100mL deionized water, add 0.5g dried cellulose sample, stir well, and adjust the pH to 10. Add 40mmol / g NaClO solution for oxidation, stir evenly at 500rpm with a magnetic stirrer at room temperature, and continuously add 0.5mol / L NaOH during the oxidation process to maintain the pH of the reaction system between (10±0.2). When the pH is stable and no longer changes (about 3-4h), add 10mL ethanol to terminate the reaction, and adjust the pH to neutral with 0.5mol / L HCl. The lower precipitate was removed by centrifugation (1000 rpm, 10 min) and rinsed three times with ethanol (95% by volume) and deionized water to remove excess salt and impurities. The precipitate was then dispersed in 200 mL of deionized water again and homogenized 10 times in a high-pressure homogenizer at a pressure of 600 bar. The obtained nanocellulose solution was freeze-dried to obtain cellulose nanofibers.

[0070] In S3, 6% (w / v) kafirin and 2.5% (v / v) polyethylene glycol (PEG-300) were dissolved in 70% ethanol aqueous solution and stirred at 70°C for 1 h under a magnetic stirrer. 0.5% cellulose nanofibers were added to the solution and continued to stir at 70°C for 1 h. The mixture was homogenized at 12000 rpm for 10 min and ultrasonicated for 10 min. The cellulose nanofiber-kafirin mixture was cast on a mold using a solution casting method and kept in an oven at 60°C for 8 h. The dried film was removed from the oven and cooled at room temperature, and the cast film was gently lifted from the mold to obtain a cellulose nanofiber-kafirin composite film.

[0071] Example 3

[0072] Step 6) in S1: alkaline hydrolysis: add deionized water at a material-liquid ratio of 1:10, and add 4% NaOH by mass, perform alkaline hydrolysis at 60°C for 3h, and perform ultrasonic-assisted extraction for 30min, remove the supernatant by centrifugation, and collect the precipitate. The other steps are the same as those in S1 in Example 1.

[0073] Accurately weigh 0.016g TEMPO (0.1mmol) and 0.1g NaBr (1mmol) in S2 and dissolve in 100mL deionized water, add 0.5g dried cellulose sample, stir well, and adjust pH to 10. Add 25mmol / g NaClO solution for oxidation, stir evenly at 500rpm with a magnetic stirrer at room temperature, and continuously add 0.5mol / L NaOH during the oxidation process to maintain the pH of the reaction system between (10±0.2). When the pH is stable and no longer changes (about 3-4h), add 10mL ethanol to terminate the reaction, and adjust the pH to neutral with 0.5mol / L HCl. The lower precipitate was removed by centrifugation (1000 rpm, 10 min) and rinsed three times with ethanol (95% by volume) and deionized water to remove excess salt and impurities. The precipitate was then dispersed in 200 mL of deionized water again and homogenized 10 times in a high-pressure homogenizer at a pressure of 500 bar. The obtained nanocellulose solution was freeze-dried to obtain cellulose nanofibers.

[0074] In S3, 6% (w / v) kafirin and 2.5% (v / v) polyethylene glycol (PEG-300) were dissolved in 70% ethanol aqueous solution and stirred at 70°C for 1 h under a magnetic stirrer. 1% cellulose nanofibers were added to the solution and continued to stir at 70°C for 1 h. The mixture was homogenized at 12000 rpm for 10 min and ultrasonicated for 10 min. The cellulose nanofiber-kafirin mixture was cast on a mold using a solution casting method and kept in an oven at 60°C for 8 h. The dried film was removed from the oven and cooled at room temperature, and the cast film was gently lifted from the mold to obtain a cellulose nanofiber-kafirin composite film.

[0075] Comparative Example 1

[0076] The difference between this embodiment and Example 1 is that the oxidation concentration of NaClO in S2 is changed to 10 mmol / g, and the other steps are the same as those in Example 1. All the embodiments and all the comparative examples use vinasse from the same source and the same batch.

[0077] Comparative Example 2

[0078] The difference between the above method and Example 1 is that the concentration of cellulose nanofibers added to S3 is 0%, and the other steps are the same as those in Example 1.

[0079] Comparative Example 3

[0080] The difference between this method and Example 1 is that the concentration of cellulose nanofibers added in S3 is 1.5%, and the other steps are the same as those in Example 1.

[0081] Experimental Example 1. Infrared spectroscopy analysis of cellulose and CNF25

[0082] The chemical structure of the samples was analyzed by infrared spectroscopy, with a wave number range of 600-4000cm -1 , the spectrometer resolution is 4cm -1 , the signal-to-noise ratio is 50000:1, and the scans are 64 times.

[0083] like Figure 1 As shown in the figure, cellulose and CNF25 showed similar infrared spectra, indicating that the oxidized cellulose nanofibers did not change the basic structure of cellulose. -1 The peak at 2891cm is the stretching vibration peak of OH. With the increase of oxidation concentration, the peak width and peak intensity gradually increase. -1 It is the CH stretching vibration peak. 1607cm -1 It is the carboxyl absorption peak, which is because the hydroxyl groups of cellulose are oxidized to carboxyl groups under the action of oxidants. -1 It is the -CH2 and CH bending vibration peak. 1046cm -1 、878cm -1 It is the characteristic peak of cellulose pyran ring, which is generated by the vibration of COC and CH skeleton. -1 and 1502cm -1 Cellulose has two unique characteristic peaks, 1697 cm -1 It is caused by the vibration of residual lignin and hemicellulose carbonyl group, 1502cm -1 It is caused by the stretching vibration of the C=C double bond in lignin. After cellulose is oxidized, lignin and hemicellulose are effectively removed, so the peak of cellulose nanofibers at this wavelength disappears.

[0084] 2. XRD analysis of cellulose and CNF25

[0085] The crystal structure and compatibility of cellulose and CNF25 can be observed by XRD. Figure 2 It can be seen that when 2θ is 16° and 22.3°, there are obvious diffraction peaks, representing the (101) and (002) crystal planes of cellulose type I structure, respectively. After cellulose is TEMPO oxidized and homogenized under high pressure, the crystal structure of cellulose is not destroyed, which is consistent with the FTIR results. The many miscellaneous peaks of cellulose are caused by the residual hemicellulose and lignin in the non-crystalline area of ​​cellulose. According to the sega l formula, the crystallinity of cellulose and CNF25 is 59.3% and 65.8% respectively. After oxidation, the hemicellulose and lignin in the non-crystalline area are hydrolyzed and dissolved, thereby increasing the crystallinity.

[0086] 3. Macroscopic morphology and particle size of CNF10 and CNF25

[0087] As shown in Figure 3 (A), the suspension formed by CNF10 is relatively viscous and the system is opaque, but the overall dispersion is relatively uniform and no precipitation occurs. The CNF25 liquid is clear and transparent, no cellulose particles can be seen, and the dispersion is stable. This shows that the cellulose after TEMPO-high-pressure homogenization exhibits good water dispersibility. With the increase of oxidation concentration, the carboxyl content increases, which increases the dispersion stability of cellulose nanofibers. As shown in Figure 3 (B), the average particle size of one peak of CNF10 is 122nm, and the average particle size of the other peak is about 396nm, indicating that the dispersion system is not uniform enough. The peak of CNF25 is around 122nm. This is because as the oxidation concentration increases, more hydroxyl groups in the cellulose molecules are oxidized to carboxyl groups, and the repulsion between the negative charges of the carboxyl groups promotes the separation of cellulose and makes the fibers loose. On the other hand, the strong electrostatic repulsion generated by cellulose nanofibers also promotes defibrillation during high-pressure homogenization, further promoting the production of shorter nanofibers.

[0088] 4. Infrared spectroscopy analysis of kafirin film and composite film

[0089] The chemical structure of the samples was analyzed by infrared spectroscopy, and the ATR mode was used for analysis and determination, with a wave number range of 600-4000cm -1 , the spectrometer resolution is 4cm -1 , the signal-to-noise ratio is 50000:1, and the scans are 64 times.

[0090] The results are as follows Figure 4 The amide I band (C=O stretching vibration), amide II band (NH bending vibration) and amide III band (NH and CN stretching and bending) are at 1652, 1541 and 1097 cm, respectively. -1 3287cm -1 The peak at 2925cm belongs to the bending vibration of OH and NH. -1 The peak at 1652 and 1634 cm belongs to the stretching vibration of -CH2. The natural sorghum protein is mainly α-helical, but -1 The change in peak intensity at 1556 cm-1 may indicate a structural transition from native protein to condensed protein. -1 However, after adding cellulose nanofibers, the amide II band absorption shifted to 1542 cm -1 This indicates that a small amount of molecular bonding occurred between the amino groups of kafirin and the carboxyl groups of nanocellulose, and there was a cross-linking effect between cellulose nanofibers and kafirin.

[0091] 5. Surface morphology and cross section of composite membrane

[0092] Surface morphology and cross-section of the fractured area of ​​cellulose nanofiber-kafirin composite film Figure 5 As shown. When only kafirin was added, irregular holes existed on the membrane surface, but as the amount of cellulose nanofibers added increased, the holes decreased, the membrane thickness decreased, and the surface became smooth. This is because cellulose nanofibers are biocompatible and can be more evenly dispersed in kafirin. The dispersion of cellulose nanofibers in the composite membrane is due to the similar charges between them. The numerous hydroxyl groups from kafirin and cellulose nanofibers can provide good miscibility with each other through hydrogen bonds and electrostatic interactions. When the cellulose nanofiber addition amount was 1%, the membrane thickness was 47.6 μm and the surface was smooth. However, when the addition amount was 1.5%, the excess cellulose nanofibers would agglomerate, which would lead to phase separation between the nanofibers and the matrix. The surface morphology and cross-section of the composite membrane became rough, which is also the reason for the decline in various performance indicators of the composite membrane.

[0093] Experimental Example 2 Performance Test of Cellulose Nanofiber-Kafirin Composite Film

[0094] 1. Analysis of thermal stability of kafirin film and composite film

[0095] Thermogravimetric analysis is an effective method to study the thermal degradation of materials. It provides a more comprehensive understanding of the application of composite membranes. The TGA curve of cellulose nanofiber-kafirin composite membrane is shown in Figure 2. Figure 6 As shown in the figure, the pure kafirin film begins to decompose at 225°C. After kafirin is cross-linked with 1% cellulose nanofibers, the thermal decomposition temperature of the composite film increases and it begins to decompose at 241°C, showing good thermal stability. This is because the carboxyl groups of the cellulose nanofibers and the amino groups of the protein have a strong interaction, which improves the thermal stability.

[0096] 2. Composite film transmittance test

[0097] In order to further study the transmittance of cellulose nanofiber-kafirin composite film, the transmittance analysis was carried out by UV spectroscopy. Figure 7 It can be found that the light transmittance of the pure sorghum alcohol-soluble protein film is the worst, and the light transmittance of the composite film increases with the increase of the proportion of cellulose nanofibers added, indicating that cellulose nanofibers can improve the light transmittance of the protein film. The reason is that nano-scale fibers do not scatter light. Generally speaking, when the size of the components in the film is less than one-tenth of the wavelength of visible light, they will hardly scatter light. 600When the amount of cellulose nanofibers added was 1%, the transmittance of the protein film was 48.5%, and when the amount of cellulose nanofibers added was 1%, the transmittance was 60.8%. When the amount of cellulose nanofibers added was 1.5%, the transmittance was 66.7%. With the increase of cellulose nanofibers, the transmittance of the composite film increased significantly.

[0098] 3. Mechanical properties test of composite membrane

[0099] In order to further explore the mechanical strength of the composite film, the tensile strength and elongation at break of the composite film were tested. Figure 8 As shown in the figure, in general, with the increase of cellulose nanofiber addition, the tensile strength increases and the elongation at break decreases. When no cellulose nanofibers are added, the tensile strength of the film is 4.49MPa, the elongation at break is 61.9%, and it is easy to deform. When 1% of cellulose nanofibers are added, the tensile strength is the largest, which is 9.17MPa, the elongation at break is 37.4%, and the elongation at break is the lowest. Compared with the pure kafirin film without CNFs, the tensile strength is increased by 104%. The elongation at break is reduced by 40%. It has excellent deformation resistance and toughness. This is because with the increase of cellulose nanofiber addition, cross-linking occurs between cellulose nanofibers and kafirin chains, and the high aspect ratio of cellulose nanofibers makes it easier for free carboxyl groups to combine with kafirin amino groups, which increases the tensile strength. When the amount of cellulose nanofibers continues to increase, aggregation occurs between the fibers, which reduces the tensile strength and increases the elongation at break.

[0100] It will be understood by those skilled in the art that, unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as generally understood by those skilled in the art in the art to which the present invention belongs. It should also be understood that terms such as those defined in general dictionaries should be understood to have meanings consistent with the meanings in the context of the prior art, and will not be interpreted with idealized or overly formal meanings unless specifically defined as herein.

[0101] It should be understood that the detailed description of the technical solutions of the present invention by means of the preferred embodiments is illustrative rather than restrictive. A person skilled in the art may modify the technical solutions described in the embodiments, or replace some of the technical features by equivalents, based on reading the specification of the present invention; and these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a cellulose nanofiber-prolamin composite film, It is characterized in that The steps include: 1) Drying and crushing the wine lees, and extracting alcohol-soluble protein by alcohol-alkali method; using the remaining precipitate after extracting alcohol-soluble protein, extracting cellulose by ultrasonic alkali method; 2) preparing cellulose nanofibers by TEMPO oxidation (2,2,6,6-tetramethylpiperidin-1-oxyl free radical) combined with high pressure homogenization of the cellulose obtained in step 1); 3) The cellulose nanofibers prepared in step 2) are mixed with the kafirin prepared in step 1), and a cellulose nanofiber-kafirin composite film is prepared by a solution casting method.

2. The method according to claim 1, It is characterized in that The lees are fresh lees or thawed frozen liquor lees; The extracted prolamins include kafirin; Preferably, the powder is screened, degreased and desugared after being crushed.

3. The method according to claim 1, It is characterized in that The cellulose was extracted and treated with NaClO 2 Bleaching the cellulose and freeze-drying it to obtain cellulose powder; In step (2), during the TEMPO oxidation process, NaClO is the oxidant, and TEMPO and NaBr are the catalysts; In step 1), the mesh number of the sieve is 40 mesh; in the degreasing process, n-hexane is used for degreasing, wherein the ratio of vinasse powder to n-hexane is 1 g:10 mL; Adding xylanase, thermostable α-amylase and glucosidase to the material to enzymatically hydrolyze the polysaccharide in the material, and removing low molecular weight soluble sugar after enzymatic hydrolysis by centrifugation; The enzymatic hydrolysis temperature of the xylanase is 50-60°C, the pH is 5.5-6.0, and the enzyme activity is 60 U / g; The enzymatic hydrolysis temperature of the thermostable α-amylase is 40-55°C, the pH is 5.5-6.5, and the enzyme activity is 2000 U / g; The enzymatic hydrolysis temperature of the glucanase is 50-55° C., the pH is 6.0-6.5, and the enzyme activity is 500 U / g.

4. The method according to claim 1, It is characterized in that The centrifugal force used in the centrifugation is 1000-12000 rpm, the centrifugal temperature is 4-25°C, the centrifugal time is 10-15 min, and the supernatant is removed; In step 1), the ethanol concentration is 65-75%, and the base is NaOH; In step 1), the concentration of sodium metabisulfite in the alcohol-alkali method is 5 g / L, and the concentration of NaOH is 3-3.5 g / L; The conditions of the alkalization by ultrasonic alkali method in step 1) include: reaction time 3-5 h, reaction temperature 50-70° C.; NaOH mass fraction: 2-4%; In step 1), the ultrasonic alkali method is performed for an ultrasonic time of 10-30 min; In step 2), the NaClO oxidation concentration is 25-40 mmol / g, the pH is 9.8-10.2, the high-pressure homogenization pressure is 500-600 bar, and the cycle is repeated 10 times.

5. The method according to claim 1, It is characterized in that Preferably, in step 3), the concentration of kafirin is 5%-7% (w / v), and the concentration of cellulose nanofibers is 0%-1.5%.

6. A cellulose nanofiber-prolamin composite film, It is characterized in that The compound is prepared by the preparation method according to any one of claims 1 to 5.

7. The composite film according to claim 6, It is characterized in that When the addition amount of cellulose nanofibers was 1%, the thickness of the cellulose nanofiber-kafirin composite film was 47.6 μ m, compared with the protein film, the thickness is reduced and the surface becomes smoother.

8. The composite film according to claim 6, It is characterized in that When the addition amount of cellulose nanofibers is 1%, the maximum tensile strength of the cellulose nanofiber-kafirin composite film is 9.17 MPa, which is 104% higher than that of the protein film.

9. The composite film according to claim 6, It is characterized in that When the addition amount of cellulose nanofibers was 1%, the decomposition temperature of the cellulose nanofiber-kafirin composite film was 225℃, and the decomposition temperature of the protein film was 241℃. The composite film showed better thermal stability.

10. Use of a cellulose nanofiber-prolamin composite film in green packaging, wherein the composite film is any one of claims 6 to 9, or is prepared by the preparation method of any one of claims 1 to 5.

Citation Information

Cited By

  • Preparation and application of vinasse araboxylan-sorghum prolamin compound

    CN121401151A