Rubber composition for sheet conveyance roller, and sheet conveyance roller
By adding terpene-based resin to the rubber composition of the sheet conveying roller and mixing at a specific temperature, the problem of insufficient friction coefficient of the sheet conveying roller in the prior art is solved, and a more efficient sheet conveying performance is achieved.
Patent Information
- Application Number
- CN202311795143.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-06-02
- Filing Date
- 2023-12-25
- Publication Date
- 2024-12-03
AI Technical Summary
The existing sheet conveying rollers are prone to wear when sending single sheets at high speed, and are difficult to maintain a high coefficient of friction, which affects the conveying efficiency.
A terpene-based resin is added to a base material containing a diene rubber, and the rubber composition is formed to increase the friction coefficient by mixing it at a temperature above the softening point of the terpene-based resin.
The friction coefficient of the sheet conveying roller is significantly improved, and the conveying performance in the wear state is enhanced. It is particularly suitable for document processing devices for scanning or classification.
Smart Images

Figure CN119060425A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a rubber composition for forming a sheet conveying roller. Background Art
[0002] Various sheet conveying rollers are assembled in sheet conveying mechanisms of electrostatic copiers, laser printers, plain paper fax machines and their combined machines, image forming devices such as inkjet printers, and automatic teller machines (ATMs). The sheet conveying rollers rotate while contacting sheets such as paper and plastic films, and convey the sheets by friction.
[0003] As the material of the sheet conveying roller, ethylene-propylene-diene monomer copolymer (EPDM) is often used from the viewpoints of friction coefficient, environmental resistance (ozone resistance, etc.), cost, etc. Here, in recent years, the types of sheets used in image forming devices, etc. have become more diverse, and there are cases where a high friction coefficient is required for the sheet conveying roller. In particular, the roller for conveying single sheets used in a document processing device that scans or sorts bills is easy to wear because it feeds a variety of single sheets at high speed, and maintains a high friction coefficient even in a worn state. Therefore, various technologies for increasing the friction coefficient of the roller have been proposed.
[0004] For example, Patent Document 1 describes a rubber composition for forming a roller body of a paper feed roller, the rubber composition comprising: a rubber containing at least ethylene-propylene-diene rubber, 20 parts by mass or less of a filler relative to 100 parts by mass of the total amount of the rubber, and 2.5 parts by mass or more of a peroxide cross-linking agent relative to 100 parts by mass of the total amount of the rubber, the ethylene-propylene-diene rubber being a non-oil-extended ethylene-propylene-diene rubber and an oil-extended ethylene-propylene-diene rubber each having an ethylene content of 55% or more and 72% or less, and the proportion of the non-oil-extended ethylene-propylene-diene rubber being 20 parts by mass or more and 80 parts by mass or less in 100 parts by mass of the total amount of the rubber.
[0005] In addition, Patent Document 2 describes a paper feed roller, which includes a roller body, the roller body being formed of a cross-linked product of a rubber composition, the rubber composition containing at least one isoprene-based rubber selected from isoprene rubber and natural rubber (excluding epoxidized natural rubber) in a ratio of 55 parts by mass or more based on 100 parts by mass of the total amount of rubber. [Prior art literature] [Patent Document]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 2020-02271 [Patent Document 2] Japanese Patent Application Publication No. 2021-91549 Summary of the invention [Problems to be solved by the invention]
[0007] An object of the present invention is to provide a rubber composition which improves the friction coefficient of a sheet conveying roller. [Methods used to solve the problem]
[0008] The inventors of the present invention have already proposed that a sheet conveying roller having an excellent friction coefficient can be produced by a rubber composition in which a terpene resin is added to a base rubber containing EPDM, but after further research to seek a further improvement in the friction coefficient, they found that the friction coefficient of the sheet conveying roller produced by adding a terpene resin to a base rubber containing a diene rubber can be further improved, thereby completing the present invention. That is, the rubber composition for a sheet conveying roller of the present invention that can solve the above-mentioned problems is characterized in that it contains a base rubber and a terpene resin, and the base rubber contains a diene rubber. [Effects of the invention]
[0009] According to the present invention, it is possible to provide a sheet conveying roller having an improved friction coefficient. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figure 1 It is a perspective view showing an example of the sheet conveying roller of the present invention. Figure 2 It is a schematic diagram explaining the method of measuring the friction coefficient. [Explanation of symbols] 1: Sheet conveying roller, 2: Roller body, 3: Through hole, 4: Shaft, 10: Plate, 11: Paper, 12: Load cell DETAILED DESCRIPTION
[0011] <Rubber composition for sheet conveying roller> The rubber composition for a sheet conveying roller of the present invention (hereinafter, sometimes simply referred to as “rubber composition”) contains a diene rubber as a base rubber and a terpene resin.
[0012] (Base rubber) The rubber composition contains a diene rubber as a base rubber. The diene rubber is not particularly limited as long as it is a polymer containing a diene compound as a main component, and may be a polymer formed by a diene compound (a homopolymer formed by one diene compound, or a copolymer formed by multiple diene compounds), or a copolymer formed by a diene compound and a non-diene compound. These diene rubbers may be used alone or in combination of two or more.
[0013] Examples of the diene compound include isoprene, chloroprene, butadiene, pentadiene, etc. The diene compound may be used alone or in combination of two or more thereof. In addition, a conjugated diene compound is preferably used as the diene compound.
[0014] Examples of the non-diene compound include styrene, acrylonitrile, ethylene, propylene, etc. The non-diene compound may be used alone or in combination of two or more.
[0015] Specific examples of the diene rubber include natural rubber (NR), isoprene rubber (IR), styrene-butadiene rubber (SBR), butadiene rubber (BR), acrylonitrile-butadiene rubber (NBR), chloroprene rubber (CR), etc. Among them, natural rubber, isoprene rubber, and styrene-butadiene rubber are preferred from the viewpoint of further improving the friction coefficient, and natural rubber and isoprene rubber are more preferred.
[0016] Natural rubber is derived from plants containing rubber and contains pure cis-1,4-polyisoprene. As the natural rubber, for example, various natural rubbers such as SMR (standard Malaysian rubber), SVR (standard Vietnamese rubber), SIR (standard Indonesian rubber), STR (standard Thai rubber), SSR (standard Singapore rubber), SCR (standard Ceylon rubber) classified according to the origin, and various sheet rubbers such as ribbed smoked rubber sheets (Ribbed Smoked Sheet), white crepe sheets (whitecrepe), pale crepe, estate brown crepe sheets (estate brown crepe), compocrepe, thin brown crepe sheets (thin brown crepe), and thick brown crepe sheets (thick brown crepe) in the variety grades classified according to the Green Book can be listed. In addition, as the natural rubber, modified natural rubbers such as deproteinized natural rubber, hydrogenated natural rubber, and grafted natural rubber can also be listed. These natural rubbers can be used alone, or two or more can be used in combination. In addition, in the present invention, as natural rubber, it is particularly preferred to use unmodified natural rubber.
[0017] Isoprene rubber is a rubber that artificially reproduces the structure of natural rubber. Examples of the isoprene rubber include various types of isoprene rubber classified according to Mooney viscosity.
[0018] In the diene rubber, the content of the structural unit derived from the diene compound is preferably 50% by mass or more, more preferably 60% by mass or more, further preferably 80% by mass or more, and particularly preferably 90% by mass or more. In addition, the upper limit of the content is 100% by mass. When the content of the structural unit derived from the diene compound is within the above range, the friction coefficient of the roller is further improved.
[0019] The base rubber preferably contains the diene rubber as a main component. The content of the diene rubber in 100% by mass of the base rubber is preferably 50% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more. In addition, in the present invention, it is also a preferred embodiment to contain only the diene rubber as the base rubber. When the content of the diene rubber is within the above range, the friction coefficient of the roller is further improved.
[0020] In the rubber composition of the present invention, as a base rubber, in addition to the diene rubber, a non-diene rubber may also be contained. As for the non-diene rubber, as a constituent component, as long as it is a polymer containing a non-diene compound as the main body, there is no particular limitation, for example, ethylene-α-olefin copolymers, ethylene-vinyl acetate copolymers, epichlorohydrin rubbers, acrylic rubbers, butyl rubbers, silicone rubbers, etc. can be cited. These non-diene rubbers can be used alone or in combination of two or more. Among them, from the viewpoint of improving ozone resistance, ethylene-α-olefin copolymers and ethylene-vinyl acetate copolymers are particularly preferred.
[0021] Ethylene-α-olefin copolymers are copolymers containing at least ethylene and α-olefin as constituent components. In addition, the ethylene-α-olefin copolymers also include ethylene-α-olefin-diene copolymers in which double bonds are introduced into the main chain by adding a small amount of diene components to ethylene and α-olefin. The ethylene-α-olefin copolymers may be used alone or in combination of two or more.
[0022] Examples of the α-olefin include propylene, 1-butene, 1-hexene, and 1-octene.
[0023] Examples of the diene component include ethylidene norbornene (ENB), 1,4-hexadiene (1,4-HD), and dicyclopentadiene (DCP), and ethylidene norbornene is preferred.
[0024] Examples of the ethylene-α-olefin copolymer include ethylene-propylene copolymer (EPM), ethylene-butene copolymer (EBR), ethylene-octene copolymer (EOR), etc. In addition, examples of the ethylene-α-olefin-diene copolymer include ethylene-propylene-diene copolymer (EPDM), ethylene-butene-diene copolymer (EBDM), ethylene-propylene-butene-diene copolymer (EPBDM), etc.
[0025] The content of the ethylene component of the ethylene-α-olefin copolymer is preferably 40% by mass or more, more preferably 42% by mass or more, further preferably 43% by mass or more, and in addition, preferably 79% by mass or less, more preferably 78% by mass or less, further preferably 77% by mass or less. When the content of the ethylene unit is within the above range, commercial products are easily obtained, and rubber suitable for sheet conveying rollers can be obtained.
[0026] When the ethylene-α-olefin-diene copolymer is used as the ethylene-α-olefin copolymer, the content of the diene component is preferably 0.5% by mass or more, more preferably 0.7% by mass or more, and further preferably 1.0% by mass or more, and preferably 15% by mass or less, more preferably 14% by mass or less, and further preferably 13% by mass or less. When the content of the diene unit is within the above range, commercial products are easily obtained, and a rubber suitable for use as a sheet conveying roller can be obtained.
[0027] The ethylene-α-olefin copolymer includes an oil-extended ethylene-α-olefin copolymer whose softness is adjusted by adding an extender oil, and a non-oil-extended ethylene-α-olefin copolymer without adding an extender oil, either of which can be used. In addition, in the case of the oil-extended type, the mass of the added extender oil is treated as a processing aid.
[0028] Ethylene-vinyl acetate copolymer is a copolymer containing ethylene and vinyl acetate as constituent components. The content of the ethylene component of the ethylene-vinyl acetate copolymer is preferably 5% by mass or more, more preferably 7% by mass or more, and further preferably 10% by mass or more, and is preferably 70% by mass or less, more preferably 60% by mass or less, and further preferably 50% by mass or less. This is because when the content of the ethylene unit is within the above range, a commercial product is easily obtained.
[0029] When the base rubber contains the ethylene-α-olefin copolymer and / or the ethylene-vinyl acetate copolymer, the content of the ethylene-α-olefin copolymer and the ethylene-vinyl acetate copolymer in 100% by mass of the base rubber is preferably 25% by mass or more, more preferably 30% by mass or more, and further preferably 35% by mass or more, and preferably less than 50% by mass, more preferably 48% by mass or less, and further preferably 45% by mass or less. When the content of the ethylene-α-olefin copolymer and the ethylene-vinyl acetate copolymer is within the above range, a high friction coefficient can be maintained and ozone resistance can be improved.
[0030] (Terpene resin) The rubber composition for a sheet conveying roller of the present invention contains a terpene resin. By containing the terpene resin, the friction coefficient of the sheet conveying roller can be increased.
[0031] The terpene resin is not particularly limited as long as it is a polymer having a terpene compound as a constituent component. Examples of the terpene resin include terpene resins, aromatic modified terpene resins, and hydrogenated products thereof. These terpene resins may be used alone or in combination of two or more.
[0032] The terpene resin is a homopolymer obtained by polymerizing a terpene compound. The terpene compound is (C5H8) n The hydrocarbons and their oxygenated derivatives are classified as monoterpenes (C 10 H 16 ), sesquiterpenes (C 15 H 24 ), diterpenes (C 20 H 32 ) and the like as a basic skeleton. Examples of the terpene compound include α-pinene, β-pinene, dipentene, limonene, myrcene, alloocimene, ocimene, α-phellandrene, α-terpinene, γ-terpinene, terpinolene, 1,8-cineole, 1,4-cineole, α-terpineol, β-terpineol, γ-terpineol, and the like. The terpene compound may be used alone or in combination of two or more thereof.
[0033] Examples of the terpene resin include α-pinene polymers, β-pinene polymers, limonene polymers, dipentene polymers, and β-pinene / limonene polymers.
[0034] The aromatic modified terpene resin is a copolymer of the terpene compound and an aromatic compound. Examples of the aromatic modified terpene resin include terpene phenol resin, terpene styrene resin, terpene phenol styrene resin, and the like.
[0035] The terpene phenol resin is, for example, a copolymer of the terpene compound and a phenolic compound. Examples of the phenolic compound include phenol, cresol, xylenol, catechol, resorcinol, hydroquinone, bisphenol A, and the like. The terpene phenol resin is preferably a copolymer of a terpene compound and phenol.
[0036] The terpene styrene resin is, for example, a copolymer of the terpene compound and a styrene-based compound. Examples of the styrene-based compound include styrene and α-methylstyrene. The terpene styrene resin is preferably a copolymer of the terpene compound and α-methylstyrene.
[0037] The terpene phenol styrene resin is, for example, a copolymer of the terpene compound, the phenol compound and the styrene compound. As the terpene phenol styrene resin, a copolymer of the terpene compound, phenol and α-methylstyrene is preferred.
[0038] In addition, the terpene resin may be a hydrogenated terpene resin obtained by adding hydrogen atoms to the above-mentioned terpene resin or aromatic modified terpene resin. The double bonds in the molecule are hydrogenated by adding hydrogen atoms. The hydrogenated product may be a fully hydrogenated terpene resin in which all double bonds in the molecule are hydrogenated or a partially hydrogenated terpene resin in which part of the double bonds in the molecule are hydrogenated.
[0039] Examples of the hydrogenated terpene resin include a hydrogenated terpene resin obtained by hydrogenating the terpene resin, a hydrogenated terpene phenol resin obtained by hydrogenating the terpene phenol resin, a hydrogenated terpene styrene resin obtained by hydrogenating the terpene styrene resin, and a hydrogenated terpene phenol styrene resin obtained by hydrogenating the terpene phenol styrene resin.
[0040] The terpene-based resin is preferably at least one selected from the group consisting of terpene resins, terpene phenol resins, terpene styrene resins, terpene phenol styrene resins, hydrogenated terpene phenol resins, hydrogenated terpene styrene resins, and hydrogenated terpene phenol styrene resins.
[0041] The softening point of the terpene resin is preferably 50°C or higher, more preferably 60°C or higher, and further preferably 70°C or higher, and is preferably 150°C or lower, more preferably 140°C or lower, and further preferably 130°C or lower. When the softening point is 50°C or higher, storage and handling during measurement are easy, and when the softening point is 150°C or lower, the resin is easily softened during kneading and kneading is easy. In addition, the softening point of the terpene resin is measured according to the 7.7 softening point of JIS K6220-1 (2015).
[0042] The hydroxyl value of the terpene resin is preferably 250 mgKOH / g or less, more preferably 200 mgKOH / g or less, further preferably 150 mgKOH / g or less, particularly preferably 100 mgKOH / g or less, and most preferably 50 mgKOH / g or less. In addition, the lower limit of the hydroxyl value of the terpene resin is 0 mgKOH / g. If the hydroxyl value of the terpene resin is 250 mgKOH / g or less, the wear resistance of the obtained roller is further improved. The hydroxyl value is measured by potentiometric titration (JIS K0070 (1992)).
[0043] In the rubber composition, the content of the terpene resin is preferably 1.0 parts by mass or more, more preferably 1.5 parts by mass or more, and further preferably 2.0 parts by mass or more, and is preferably 15 parts by mass or less, more preferably 13 parts by mass or less, and further preferably 12 parts by mass or less, relative to 100 parts by mass of the base rubber. If the content of the terpene resin is 1.0 parts by mass or more, the friction coefficient of the sheet conveying roller is further improved, and if the content of the terpene resin is 15 parts by mass or less, adhesion to the inner wall of the device during kneading can be suppressed, and the processability becomes good.
[0044] (Vulcanizing agent) The rubber composition preferably contains a vulcanizing agent. By containing a vulcanizing agent, the wear resistance of the obtained sheet conveying roller is further improved. As the vulcanizing agent, sulfur-based vulcanizing agents, organic peroxides, etc. can be listed. These vulcanizing agents can be used alone or in combination of two or more.
[0045] Examples of the sulfur-based vulcanizing agent include elemental sulfur and sulfur-donor compounds. Examples of the elemental sulfur include powdered sulfur, precipitated sulfur, colloidal sulfur, and insoluble sulfur. Examples of the sulfur-donor compound include 4,4'-dithiobismorpholine.
[0046] Examples of the organic peroxide include dicumyl peroxide, α,α′-bis(tert-butylperoxy-m-diisopropyl)benzene, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, and 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane.
[0047] When the rubber composition of the present invention contains a vulcanizing agent, the content of the vulcanizing agent is preferably 0.5 parts by mass or more, more preferably 0.8 parts by mass or more, and further preferably 1.0 parts by mass or more, and preferably 5.0 parts by mass or less, more preferably 4.0 parts by mass or less, and further preferably 3.0 parts by mass or less, relative to 100 parts by mass of the base rubber. When the content of the vulcanizing agent is 0.5 parts by mass or more, the wear resistance of the roller formed is further improved, and when the content of the vulcanizing agent is 5.0 parts by mass or less, the hardness of the roller formed does not become too high, and the friction coefficient becomes better.
[0048] (Vulcanization accelerator) The rubber composition may contain a vulcanization accelerator. As the vulcanization accelerator, any of an inorganic accelerator and an organic accelerator may be used. As the inorganic accelerator, slaked lime, magnesium oxide (magnesia) (MgO), litharge (litharge) (PbO) and the like may be cited. As the organic accelerator, for example, thiuram-based accelerators, thiazole-based accelerators, sulfonamide-based accelerators, dithiocarbamate-based accelerators and the like may be cited. The vulcanization accelerator may be used alone or in combination of two or more. As a vulcanization accelerator combined with the sulfur-based vulcanizing agent, it is preferred to use a thiuram-based accelerator and a thiazole-based accelerator in combination.
[0049] Examples of the thiuram-based accelerator include tetramethylthiuram monosulfide, tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetrabutylthiuram disulfide, tetrakis(2-ethylhexyl)thiuram disulfide, and dipentamethylenethiuram tetrasulfide.
[0050] Examples of the thiazole accelerator include 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, zinc salt of 2-mercaptobenzothiazole, cyclohexylamine salt of 2-mercaptobenzothiazole, 2-(N,N-diethylthiocarbamoylthio)benzothiazole, and 2-(4′-morpholinyldithio)benzothiazole.
[0051] When the rubber composition of the present invention contains a vulcanization accelerator, the content of the vulcanization accelerator is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, and further preferably 2 parts by mass or more, and preferably 10 parts by mass or less, more preferably 8 parts by mass or less, and further preferably 6 parts by mass or less, relative to 100 parts by mass of the base rubber. If the content of the vulcanization accelerator is 0.5 parts by mass or more, the vulcanization acceleration effect is improved, and if the content of the vulcanization accelerator is 10 parts by mass or less, the physical properties of the formed roller become better.
[0052] When the thiuram accelerator and the thiazole accelerator are used together, the mass ratio (thiuram accelerator / thiazole accelerator) is preferably 0.5 or more, more preferably 1.0 or more, and even more preferably 1.2 or more, and is preferably 5 or less, more preferably 3 or less, and even more preferably 2 or less. When the mass ratio (thiuram accelerator / thiazole accelerator) is within the above range, the physical properties of the resulting roller are further improved.
[0053] (Vulcanization accelerator) The rubber composition may contain a vulcanization accelerator. Examples of the vulcanization accelerator include metal compounds such as zinc oxide, and fatty acids such as stearic acid, oleic acid, and cottonseed fatty acid. These vulcanization accelerators may be used alone or in combination of two or more.
[0054] When the rubber composition of the present invention contains a vulcanization accelerator, the content of the vulcanization accelerator is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and further preferably 5 parts by mass or more, and preferably 10 parts by mass or less, more preferably 9 parts by mass or less, and further preferably 8 parts by mass or less, relative to 100 parts by mass of the base rubber. If the content of the vulcanization accelerator is 1 part by mass or more, the effect of adding the vulcanization accelerator becomes high, and if the content of the vulcanization accelerator is 10 parts by mass or less, the physical properties of the formed roller become better.
[0055] In addition, it is also preferred to use a metal compound and a fatty acid in combination as a vulcanization accelerator. In this case, the mass ratio of the metal compound to the fatty acid (metal compound / fatty acid) is preferably 1 or more, more preferably 2 or more, further preferably 3 or more, and preferably 10 or less, more preferably 8 or less, further preferably 6 or less. When the mass ratio (metal compound / fatty acid) is within the above range, the physical properties of the formed roller become better.
[0056] When the rubber composition of the present invention contains a sulfur-based vulcanizing agent as a vulcanizing agent, it is preferred to further contain a vulcanization accelerator and / or a vulcanization accelerating aid. On the other hand, when the rubber composition of the present invention contains an organic peroxide as a vulcanizing agent, the rubber composition may not contain a vulcanization accelerator and / or a vulcanization accelerating aid.
[0057] (Other ingredients) The rubber composition may contain fillers, processing aids, antioxidants, peptizers, pigments, vulcanization retarders, etc., within the scope of not impairing the gist of the present invention. These additives may be blended as necessary.
[0058] Examples of the filler include carbon black, silica, clay, talc, calcium carbonate, magnesium carbonate, barium sulfate, etc., which are known as fillers or reinforcing materials for rubber. By adding the filler, the mechanical strength of the obtained roller can be improved.
[0059] The content of the filler is preferably 5 parts by mass or more, more preferably 8 parts by mass or more, and further preferably 10 parts by mass or more, and preferably 100 parts by mass or less, more preferably 80 parts by mass or less, and further preferably 50 parts by mass or less, relative to 100 parts by mass of the base rubber. If the content of the filler is within the above range, the physical properties of the formed roller are further improved.
[0060] Examples of the processing aid include fatty acid esters, fatty acid metal salts, fatty acid amides, hydrocarbons (paraffins), process oils, and the like.
[0061] Examples of the antioxidant include nickel diethyldithiocarbamate and nickel dibutyldithiocarbamate.
[0062] The hardness (durometer method, type A hardness) of the cured product of the rubber composition is preferably 10 or more, more preferably 15 or more, further preferably 20 or more, and preferably 90 or less, more preferably 85 or less, further preferably 80 or less. If the hardness of the cured product is 10 or more, it becomes a hardness suitable for sheet conveyance, and the conveyance force is further improved. If the hardness of the cured product is 90 or less, the roller can be pressed more easily.
[0063] <Manufacturing of Rubber Composition for Sheet Conveyor Roller> The rubber composition for sheet conveying rollers can be prepared by mixing base rubber, terpene resin, and other components as required, and kneading them using a kneader, Banbury mixer, open roll, etc. The kneading method and conditions are appropriately selected according to the production scale.
[0064] In the method for producing the rubber composition for a sheet conveying roller of the present invention, it is preferred that the base rubber containing the diene rubber and the terpene resin be kneaded at a temperature not lower than the softening point of the terpene resin.
[0065] By mixing the base rubber and the terpene resin at a temperature above the softening point of the terpene resin, the terpene resin can be uniformly mixed in the rubber. In addition, when a plurality of terpene resins are contained, the mixing is carried out at a temperature above the softening point of the terpene resin with the highest softening point. Regarding the mixing temperature, when the softening point of the terpene resin is set to T°C, the mixing temperature is more preferably T+3°C or more, and further preferably T+5°C or more. In addition, when a plurality of terpene resins are contained, the softening point of the terpene resin with the highest softening point is set to T°C. The upper limit of the mixing temperature is not particularly limited, but is generally less than 200°C.
[0066] When the rubber composition for a sheet conveying roller of the present invention contains a vulcanizing agent, the method for producing the rubber composition for a sheet conveying roller preferably comprises the following steps: a first step: kneading a base rubber containing a diene rubber and a terpene resin at a temperature not lower than the softening point of the terpene resin to obtain a kneaded product; and a second step: mixing a vulcanizing agent into the kneaded product. By having the first and second steps, the terpene resin can be uniformly dispersed in the rubber component, and scorching caused by the vulcanizing agent can be suppressed.
[0067] In the first step, the base rubber and the terpene resin are mixed to prepare a mixture. The mixing temperature (material temperature) when mixing the base rubber and the terpene resin is preferably above the softening point of the terpene resin. By mixing at a temperature above the softening point of the terpene resin, the terpene resin can be uniformly mixed in the base rubber. In addition, when a plurality of terpene resins are contained, the mixture is mixed at a temperature above the softening point of the terpene resin with the highest softening point. Regarding the mixing temperature of the first step, when the softening point of the terpene resin is set to T°C, the mixing temperature of the first step is more preferably above T+3°C, and further preferably above T+5°C. In addition, when a plurality of terpene resins are contained, the softening point of the terpene resin with the highest softening point is set to T°C. The upper limit of the mixing temperature of the first step is not particularly limited, and is usually less than 200°C.
[0068] The mixing in the first step can be performed using a kneader, a Banbury mixer, an open roll mixer or the like, and is preferably performed using a kneader.
[0069] In the first step, only the base rubber and the terpene resin may be mixed, or components other than the vulcanizing agent and the vulcanization accelerator (such as the above-mentioned vulcanization accelerating aid, filler, processing aid, antioxidant and other components) may be further mixed. In addition, in the first step, it is preferred that the vulcanizing agent and the vulcanization accelerator are not mixed.
[0070] In the second step, a vulcanizing agent is mixed with the kneaded product obtained in the first step to prepare a rubber composition. The mixing temperature (material temperature) when the kneaded product and the vulcanizing agent are mixed is preferably 30° C. or higher, more preferably 40° C. or higher, and further preferably 50° C. or higher, and is preferably 150° C. or lower, more preferably 120° C. or lower, and further preferably 100° C. or lower. If the mixing temperature is 30° C. or higher, the vulcanizing agent can be easily mixed due to the plasticization of the rubber, and when the mixing temperature is 150° C. or lower, scorching can be suppressed.
[0071] The mixing in the second step can be performed using a kneader, a Banbury mixer, an open roll mill, etc., and is preferably performed using an open roll mill.
[0072] When the rubber composition for a sheet conveying roller of the present invention contains a vulcanization accelerator, the vulcanization accelerator is preferably added in the second step. When the rubber composition contains other components such as the above-mentioned vulcanization accelerator, filler, processing aid, antioxidant, etc., these components are preferably added in the first step.
[0073] <Sheet Conveying Roller> The sheet conveying roller of the present invention is molded from the rubber composition for a sheet conveying roller of the present invention.
[0074] The shape of the sheet conveying roller may be cylindrical, columnar, polygonal cylindrical, or polygonal columnar. When the sheet conveying roller is cylindrical or polygonal cylindrical, the sheet conveying roller preferably has a shaft. The material of the shaft is not particularly limited, and may be metal, ceramic, or resin.
[0075] Figure 1 An example of a sheet conveying roller is shown in FIG. Figure 1 The sheet conveying roller 1 shown in the figure comprises: a roller body 2 obtained by forming the rubber composition for sheet conveying roller of the present invention into a cylindrical shape. A through hole 3 having a circular cross section is provided at the center of the roller body 2, and a cylindrical shaft 4 connected to a drive system (not shown) is inserted and fixed in the through hole 3. The outer peripheral surface of the roller body 2 is formed into a cylindrical shape concentric with the through hole 3 and the shaft 4.
[0076] The roller body 2 and the shaft 4 are fixed to each other so that no idling occurs, for example, by pressing the shaft 4 having an outer diameter larger than the inner diameter of the through hole 3 into the through hole 3 of the roller body 2. That is, a certain idling torque (limit torque that does not cause idling) is ensured between the two by an interference fit based on the diameter difference between the two.
[0077] The shaft 4 is formed of, for example, metal, ceramics, hard resin, etc. A plurality of roller bodies 2 may be fixed to a plurality of locations on one shaft 4 as necessary.
[0078] The roller body 2 can be manufactured by forming the rubber composition into a cylindrical shape by extrusion molding or the like and then crosslinking it by pressure crosslinking or the like; or by forming the rubber composition into a cylindrical shape by transfer molding or the like and then crosslinking it.
[0079] The roller body 2 may be ground to a predetermined surface roughness, or may be knurled, textured, etc., as required, at any time point in the above-mentioned manufacturing process. In addition, both ends of the roller body 2 may be cut so that the outer peripheral surface has a predetermined width. The outer peripheral surface of the roller body 2 may be coated with any coating.
[0080] In addition, the roller body 2 may be formed into a double-layer structure of an outer layer on the outer peripheral surface side and an inner layer on the through hole 3 side. In this case, it is preferred that at least the outer layer is formed of the rubber composition of the present invention. Among them, in consideration of simplifying the structure, improving productivity and reducing manufacturing costs, it is preferred that the roller body 2 is Figure 1 The structure shown is formed into a single layer.
[0081] The roller body 2 may be porous, but preferably the roller body 2 is substantially non-porous in order to improve wear resistance or reduce compression set so that even when the contact state at one location continues for a relatively long time, it is difficult to cause depression due to deformation.
[0082] The through hole 3 may be provided at a position eccentric from the center of the roller body 2 according to the purpose of the sheet conveying roller 1. In addition, the outer peripheral surface of the roller body 2 may be a special shape, for example, a part of the cylindrical outer peripheral surface is cut into a flat shape instead of a cylindrical shape. To manufacture the sheet conveying roller 1 having the roller body 2 of such a special shape, the roller body 2 of the special shape may be directly formed by the manufacturing method described above and then cross-linked, or the roller body 2 formed into a cylindrical shape may be formed into a special shape by post-processing.
[0083] Alternatively, the shaft 4 formed into a deformed shape corresponding to the deformed shape of the roller body 2 may be press-fitted into the through hole 3 of the roller body 2 formed into a cylindrical shape, thereby deforming the roller body 2 into the deformed shape. In this case, the outer peripheral surface 5 of the cylindrical shape before deformation can be subjected to grinding, knurling, texturing, etc., so that the processability can be improved.
[0084] <Image Forming Apparatus> The sheet conveying roller of the present invention can be assembled in various image forming devices using the electrophotographic method, such as laser printers, electrostatic copiers, plain paper fax machines, or composite devices using these. In addition, the sheet conveying roller of the present invention can also be assembled in, for example, inkjet printers or ATMs. In addition, the sheet conveying roller of the present invention can also be assembled in a document processing device that scans or sorts bills.
[0085] The sheet conveying roller of the present invention rotates while in contact with the sheet, and conveys the sheet by friction. As the sheet, single sheets such as single sheets of paper and continuous sheets such as continuous paper can be cited. The sheet conveying roller can be used as, for example, a paper feed roller, a conveying roller, a platen roller, a paper discharge roller, etc. [Example]
[0086] Hereinafter, the present invention will be described in detail by way of examples, but the present invention is not limited to the following examples, and modifications and embodiments within the scope of the gist of the present invention are included in the scope of the present invention.
[0087] [Evaluation method] (1) Hardness The hardness of the cured product of the rubber composition is measured according to JIS K6253-3 (2012). Specifically, a sheet with a thickness of 2 mm is prepared by pressing at 170° C. for 20 minutes using the rubber composition. Three sheets are overlapped so as not to be affected by the measurement substrate, etc., and the sheet is brought into contact with the pressure plate of the A-type hardness meter, and the value is read 3 seconds after the contact. In addition, the hardness is measured using a hardness meter manufactured by Polymer Meter Co., Ltd.
[0088] (2) Tensile strength and elongation at break The tensile strength and elongation at break (elongation at cut) of the cured product of the rubber composition are measured according to JIS K6251 (2017). Specifically, a rubber composition is used and pressurized at 170°C for 20 minutes to make a sheet with a thickness of 2 mm, and the sheet is punched into a dumbbell shape (dumbbell No. 3 shape, thickness of the parallel part 2 mm, initial distance between markings 20 mm) to make a test piece. The physical properties are measured using a tensile test measuring device (measurement temperature 23°C, tensile speed 500 mm / min). Then, the tensile strength is calculated by dividing the maximum tensile force recorded when the test piece is stretched until it is cut by the cross-sectional area of the test piece before the test.
[0089] (3) Friction coefficient measurement like Figure 2 As shown, plain paper 11 (manufactured by FUJIFILM Business Innovation, P paper (width 60 mm, length 210 mm)) is placed on a horizontally arranged plate 10 made of polytetrafluoroethylene (PTFE). The roller body 2 of the sheet conveying roller 1 is placed on the paper 11, and a vertical load W1 (=300 gf) is applied to the shaft 4, so that the shaft 4 is pressed against the plate 10. Next, under an environment of temperature 23° C. and relative humidity 55%, the roller body 2 was rotated at 200 rpm in the direction indicated by the dashed arrow R1 , and the conveying force F (gf) applied to the load cell 12 connected to one end of the paper 11 was measured. The initial friction coefficient μ is calculated from the measured conveying force F and the vertical load W1 (=300 gf) by using the formula (1). μ=F(gf) / W1(gf) (1)
[0090] (4) Forced wear test like Figure 2 As shown, plain paper 11 (manufactured by Fujifilm Business Innovation Co., Ltd., P paper) is placed on a horizontally arranged polytetrafluoroethylene (PTFE) plate 10. The roller body 2 of the sheet conveying roller 1 is placed on the paper 11, and a vertical load W1 (=500 gf) is applied to the shaft 4, so that the shaft 4 is pressed against the plate 10. Next, the roller body 2 was rotated continuously at 200 rpm for 10 minutes in the direction indicated by the dashed arrow R1 under an environment of a temperature of 23° C. and a relative humidity of 55%. The wear reduction rate (%) was calculated from the mass W0 (g) of the roller body 2 before the rotation and the mass W1 (g) of the roller body 2 after the rotation by the following formula (2). Wear reduction rate (%) = 100 × (W0-W1) / W0 (Formula 2)
[0091] [Preparation of rubber composition] Mix the raw materials and prepare a rubber composition so as to obtain the formula shown in Table 1 and Table 2. Specifically, first, use a kneader to mix the base rubber, terpene resin and filler to prepare a mixture. At this time, after the temperature in the kneader tank (material temperature) reaches the specified temperature, mix for 1 minute. Then, the obtained mixture is cooled, and the mixture is mixed with a vulcanizer, a vulcanization accelerator and a vulcanization accelerator aid using an open mill with a surface temperature controlled at 30°C to 50°C to prepare a rubber composition. The measurement results of the cured product of the obtained rubber composition are shown in Table 1 and Table 2.
[0092] [Table 1]
[0093] [Table 2]
[0094] The raw materials used in Tables 1 and 2 are as follows. IR: Nipol (registered trademark) IR2200 (isoprene rubber), manufactured by Japan Zeon Co., Ltd. NR: Natural rubber made in Vietnam (CV-60) SBR: Nipol (registered trademark) 1502 manufactured by Nippon Zeon Co., Ltd. (styrene-butadiene rubber, bound styrene content: 23.5% by mass) EPDM: manufactured by Sumitomo Chemical Co., Ltd., Esprene 505A (non-oil-extended EPDM) (ethylene-propylene-ethylidene norbornene copolymer, ethylene content 50% by mass, diene content 9.5% by mass) Terpene resin 1: "YSResin PX1000" manufactured by Yasuhara Chemical Co., Ltd. (terpene resin, softening point: 100° C., hydroxyl value: 0 mgKOH / g) Terpene resin 2: manufactured by Yasuhara Chemical Co., Ltd., “YS Resin TO105” (aromatic modified terpene resin, softening point 105°C, hydroxyl value 0 mgKOH / g) Terpene resin 3: manufactured by Yasuhara Chemical Co., Ltd., “YS Polyster U115” (terpene phenol resin, softening point 115° C., hydroxyl value 40 mgKOH / g) Terpene resin 4: manufactured by Yasuhara Chemical Co., Ltd., “YS Polyster K125” (terpene phenol resin, softening point 125° C., hydroxyl value 200 mgKOH / g) Terpene resin 5: manufactured by Yasuhara Chemical Co., Ltd., “YS Polyster UH115” (hydrogenated terpene phenol resin, softening point 115° C., hydroxyl value 20 mgKOH / g) Sulfur: Manufactured by Tsurumi Chemical Co., Ltd., 5% oil-based sulfur Organic peroxide: manufactured by NOF Corporation, "PERCUMYL (registered trademark) D" (diisopropylbenzene peroxide) Thiuram-based vulcanization accelerator: Ouchi Shinko Chemical Industry Co., Ltd., "Nocceler (registered trademark) TOT-N" (tetrakis (2-ethylhexyl) thiuram disulfide) Thiazole vulcanization accelerator: Ouchi Shinko Chemical Industry Co., Ltd., "Nocceler DM" (di-2-benzothiazolyl disulfide) Zinc oxide: Made by Mitsui Mining & Smelting Co., Ltd., zinc oxide No. 2 Stearic acid: Made by NOF Corporation, stearic acid "Tsubaki" Carbon black: manufactured by Tokai Carbon Co., Ltd., SEAST (registered trademark) 3 Calcium carbonate: manufactured by Bihoku Funka Kogyo Co., Ltd., BF-300
[0095] [Manufacture of sheet conveying roller] The rubber composition obtained above was formed into a cylindrical shape by transfer molding at 170°C for 30 minutes. A shaft (outer diameter 12 mm) was pressed into the cylindrical molded body, and ground using a cylindrical grinder so that the outer diameter of the rubber roller became 22 mm. The width of the rubber roller part was cut to 25 mm to produce a sheet conveying roller. The evaluation results of the obtained sheet conveying roller are shown in Tables 1 and 2.
[0096] Rubber compositions No. 1 to 4 contain diene rubber (isoprene rubber (IR)) as a base rubber, terpene resin, and sulfur as a vulcanizing agent. Rubber composition No. 5 contains diene rubber and sulfur but does not contain terpene resin. The friction coefficient of the sheet conveying roller formed of rubber compositions No. 1 to 4 is improved compared to the sheet conveying roller formed of rubber composition No. 5 not containing terpene resin.
[0097] Rubber compositions No. 6 to 9 contain diene rubber (isoprene rubber (IR)) as a base rubber, a terpene resin, and an organic peroxide as a vulcanizing agent. Rubber composition No. 10 contains diene rubber and an organic peroxide, but does not contain a terpene resin. The friction coefficient of the sheet conveying roller formed of rubber compositions No. 6 to 9 is improved compared to the sheet conveying roller formed of rubber composition No. 10 not containing a terpene resin.
[0098] Rubber compositions No. 11 to 13 contain diene rubber (natural rubber) as a base rubber, terpene resin, and sulfur as a vulcanizing agent. Rubber composition No. 14 contains diene rubber and sulfur, but does not contain terpene resin. The friction coefficient of the sheet conveying roller formed of rubber compositions No. 11 to 13 is improved compared to the sheet conveying roller formed of rubber composition No. 14 not containing terpene resin.
[0099] Rubber compositions No. 15 to 17 contain diene rubber (isoprene rubber and styrene-butadiene rubber) as base rubber, terpene resin, and organic peroxide as a vulcanizing agent. Rubber composition No. 18 contains diene rubber and organic peroxide, but does not contain terpene resin. The friction coefficient of the sheet conveying roller formed of rubber compositions No. 15 to 17 is improved compared to the sheet conveying roller formed of rubber composition No. 18 not containing terpene resin.
[0100] Rubber composition No. 19 contains diene rubber (isoprene rubber and styrene-butadiene rubber) as base rubber, ethylene-α-olefin copolymer, terpene resin and organic peroxide as vulcanizing agent. Rubber composition No. 20 contains diene rubber, ethylene-α-olefin copolymer and organic peroxide, but does not contain terpene resin. The friction coefficient of the sheet conveying roller formed of rubber composition No. 19 is improved compared with the sheet conveying roller formed of rubber composition No. 20 not containing terpene resin.
[0101] The present invention (1) is a rubber composition for a sheet conveying roller, characterized in that the rubber composition for a sheet conveying roller contains a base rubber and a terpene resin, and the base rubber contains a diene rubber.
[0102] The present invention (2) is the rubber composition for a sheet conveying roller according to the present invention (1), wherein the content of the diene rubber in 100% by mass of the base rubber is 50% by mass or more.
[0103] The present invention (3) is the rubber composition for a sheet conveying roller according to the present invention (1) or (2), wherein the diene rubber contains isoprene rubber and / or natural rubber.
[0104] The present invention (4) is a rubber composition for a sheet conveying roller according to any one of the present inventions (1) to (3), wherein the content of the terpene resin is 1 to 15 parts by mass relative to 100 parts by mass of the base rubber.
[0105] The present invention (5) is the rubber composition for a sheet conveying roller according to any one of the present inventions (1) to (4), wherein the base rubber further contains an ethylene-α-olefin copolymer.
[0106] The present invention (6) is the rubber composition for a sheet conveying roller according to any one of the present inventions (1) to (5), wherein the sheet is a single sheet of paper.
[0107] The present invention (7) is a sheet conveying roller characterized in that the sheet conveying roller is obtained by molding the rubber composition for a sheet conveying roller according to any one of the present inventions (1) to (6).
[0108] The present invention (8) is a method for manufacturing a rubber composition for a sheet conveying roller, wherein the method for manufacturing a rubber composition for a sheet conveying roller is a method for manufacturing a rubber composition for a sheet conveying roller containing a base rubber and a terpene resin, and is characterized in that the base rubber containing a diene rubber and the terpene resin are mixed at a temperature above the softening point of the terpene resin.
[0109] The present invention (9) is a method for producing a rubber composition for a sheet conveying roller, which is a method for producing a rubber composition for a sheet conveying roller containing a base rubber, a terpene resin and a vulcanizing agent, and is characterized in that it includes the following steps: Step 1: kneading a base rubber containing a diene rubber and a terpene resin at a temperature not lower than the softening point of the terpene resin to obtain a kneaded product; and Second step: mixing a vulcanizing agent into the kneaded product. [Industrial Applicability]
[0110] Since the sheet conveying roller of the present invention has an increased friction coefficient, it is expected that the conveying performance will be improved. In particular, the sheet conveying roller of the present invention can be effectively used as a roller for conveying single sheets used in a document processing device for scanning or sorting bills, which is required to maintain a high friction coefficient in a worn state.
Claims
1. A rubber composition for a sheet conveying roller, characterized in that: The rubber composition for a sheet conveying roller contains a base rubber and a terpene resin. The base rubber contains a diene rubber.
2. The rubber composition for a sheet conveying roller according to claim 1, wherein The content of the diene rubber in 100% by mass of the base rubber is 50% by mass or more.
3. The rubber composition for a sheet conveying roller according to claim 1, wherein The diene rubber includes isoprene rubber and / or natural rubber.
4. The rubber composition for a sheet conveying roller according to claim 1, wherein The content of the terpene-based resin is 1 to 15 parts by mass based on 100 parts by mass of the base rubber.
5. The rubber composition for a sheet conveying roller according to claim 1, wherein The base rubber further contains an ethylene-α-olefin copolymer.
6. The rubber composition for a sheet conveying roller according to claim 1, wherein The sheet material is a single sheet of paper.
7. A sheet conveying roller, characterized in that: The sheet conveying roller is obtained by molding the rubber composition for a sheet conveying roller according to any one of claims 1 to 6.
8. A method for producing a rubber composition for a sheet conveying roller, comprising a base rubber and a terpene resin, characterized in that: The base rubber containing the diene rubber and the terpene resin are kneaded at a temperature not lower than the softening point of the terpene resin.
9. A method for producing a rubber composition for a sheet conveying roller, comprising a base rubber, a terpene resin and a vulcanizing agent, characterized in that: Including the following processes: Step 1: kneading a base rubber containing a diene rubber and a terpene resin at a temperature not lower than the softening point of the terpene resin to obtain a kneaded product; and Second step: mixing a vulcanizing agent into the kneaded product.