MDOPE film with high heat resistance

Through the use of polyethylene and polycaprolactam blending and organic intercalation modified sericite sheet monomer, the problem of degradation of heat resistance of MDOPE films is solved, and the high thermal stability and mechanical properties of the material are improved.

CN119060433APending Publication Date: 2024-12-03JIESHOU CITY TIANHONG PACKAGING MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411193904.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

After stretching, the MDOPE film has deteriorated heat resistance and is prone to deformation or softening at high temperatures, limiting its use in certain environments.

Method used

Polyethylene and polycaprolactam blended, and organic intercalation modified sericite sheet monomer was added thereto, and intercalation modification was performed by maleic anhydride grafting and allyl cationic surfactant to increase the heat of the material. Stability and mechanical strength form a three-dimensional network structure to enhance heat resistance.

Benefits of technology

It significantly improves the heat resistance of the MDOPE film, blocks heat transfer, limits the movement of the molecular chain of the polymer matrix, reduces the adverse effects of longitudinal stretching on the material performance, and enhances the overall thermodynamic performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005015810920000081
    Figure BDA0005015810920000081
  • Figure BDA0005015810920000091
    Figure BDA0005015810920000091
  • Figure BDA0005015810920000111
    Figure BDA0005015810920000111
Patent Text Reader

Abstract

The invention discloses an MDOPE film with high heat resistance, and belongs to the technical field of polyethylene films, the MDOPE film comprises the following raw materials by mass: 75-85 parts of polyethylene, 10-15 parts of polycaprolactam, 3-5 parts of a compatilizer, 1-3 parts of an antioxidant and 6-10 parts of an organic intercalation modified sericite sheet monomer, and the surface of the organic intercalation modified sericite sheet monomer is also grafted with maleic anhydride. And the heat stability of the polycaprolactam is favorable for improving the heat resistance of the blend. Due to the addition of the organic intercalation modified sericite sheet-shaped monomer, heat transfer can be blocked, the crystallization capacity of a matrix is improved, the rigidity of the material is improved, the material is not influenced by MDO treatment, and the compatibility of the organic intercalation modified sericite sheet-shaped monomer in a blend can be improved after the maleic anhydride is grafted; and the overall heat resistance can be further improved by a three-dimensional network structure formed by mutual lap joint.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyethylene films, and in particular relates to an MDOPE film with high heat resistance. Background Art

[0002] Polyethylene film (PE film) has multiple performance characteristics such as high gloss, high transparency, high tensile strength, high impact resistance and high sealing performance. The excellent optical properties, mechanical strength and sealing properties make the PE film obtained by blow molding or casting have good practicality and applicability in the field of flexible packaging.

[0003] In order to further improve the optical and barrier properties of PE film, mechanical direction orientation (MDO) is performed after PE film extrusion to change the molecular morphology of PE film. The barrier property and transparency of the obtained MDOPE film are better than the film directly rolled after co-extrusion. However, after stretching, the heat resistance of MDOPE film decreases, and it is easy to deform or soften at high temperature, which limits the use of MDOPE film in some environments. Summary of the invention

[0004] The object of the present invention is to provide a MDOPE film with high heat resistance to solve the problem of decreased heat resistance of the MDOPE film.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] The present invention provides an MDOPE film with high heat resistance, wherein the MDOPE film comprises the following raw materials in parts by weight:

[0007] 75-85 parts of polyethylene;

[0008] 10-15 parts of polycaprolactam;

[0009] 3-5 parts of compatibilizer;

[0010] 1 to 3 parts of antioxidant;

[0011] 6 to 10 parts of organic intercalation modified sericite flake monomer;

[0012] Maleic anhydride is also grafted on the surface of the organic intercalation modified sericite flake monomer.

[0013] Preferably, the compatibilizer includes one or a combination of maleic anhydride grafted compatibilizer and acrylic acid type compatibilizer.

[0014] More preferably, the maleic anhydride compatibilizer includes one or more combinations of polyethylene grafted maleic anhydride, high-density polyethylene grafted maleic anhydride, ethylene-octene copolymer grafted maleic anhydride, and ethylene-vinyl acetate copolymer grafted maleic anhydride.

[0015] More preferably, the acrylic compatibilizer includes polyethylene-glycidyl methacrylate, acrylic acid-grafted polyethylene, or a combination of both.

[0016] Preferably, the antioxidant is one or a combination of two of a phenolic antioxidant and a phosphite antioxidant.

[0017] More preferably, the phenolic antioxidant includes a combination of one or more of antioxidant 1010, antioxidant 1076, antioxidant 1098, and antioxidant 1024.

[0018] More preferably, the phosphite antioxidant includes a combination of one or more of antioxidant 168, antioxidant PEP-36, and antioxidant 618.

[0019] By adopting the above technical solution, the polyethylene film after longitudinal stretching changes its internal crystallinity and molecular orientation, resulting in poor heat resistance of the obtained MDOPE film. The raw materials of the MDOPE film of the present invention are PE (polyethylene) and PA6 (polycaprolactam) blended. Polycaprolactam has better heat resistance than polyethylene. After blending, the overall heat resistance can be improved. Under the improvement of the compatibilizer, PA6 particles are evenly dispersed in the PE matrix. PA6 as a dispersed phase can help improve the crystallization behavior of PE and enhance the thermal stability of the material.

[0020] At the same time, the present invention also adds organic intercalation modified sericite flake monomers, which are nano-scale composite materials. In addition to being able to improve the mechanical strength of the material, the sericite itself has excellent heat resistance, and the high aspect ratio of its flake crystal structure can significantly improve the thermodynamic properties of the material by virtue of high surface activity and the preferential positioning characteristics of long crystals. The nano-scale flake monomer structure also enables the sericite to be oriented along the plane direction of the film during the directional stretching in the mechanical direction, without destroying the crystal structure of the sericite, and thus will not affect the improvement effect of the sericite on the material. After the organic intercalation modification, the binding effect between the sericite flake monomer and the matrix is ​​improved, and the affinity between the flake and the polymer molecular chain is enhanced. The introduction of maleic anhydride molecules also improves the interface interaction between the sericite flake monomer and polycaprolactam, so that the organic intercalation modified sericite flake monomer can be evenly dispersed in the blended material, serving as a mechanical connection bridge of the blend, and improving the overall performance.

[0021] Preferably, the polyethylene is medium-density polyethylene and high-density polyethylene in a mass ratio of (60-80):(20-40).

[0022] By adopting the above technical scheme, the polyethylene of the present invention is blended with medium-density polyethylene and high-density polyethylene, which can increase the density of the raw material matrix while maintaining the optical properties of the material. The increase in the raw material density can minimize the adverse effects on the material during longitudinal stretching.

[0023] Preferably, the raw materials of the organic intercalation modified sericite flake monomers include sodium sericite, allyl cationic surfactant and maleic anhydride in a mass ratio of 1:(1.2-1.8):(0.4-0.6).

[0024] Preferably, the allyl cationic surfactant includes a combination of one or more of hexadecyl dimethyl allyl ammonium chloride, dodecyl dimethyl allyl ammonium chloride, octadecyl dimethyl allyl ammonium chloride, allyl trimethyl ammonium bromide, and diallyl dimethyl ammonium chloride.

[0025] Preferably, the cation exchange capacity (CEC) of sodium sericite is 35 to 40 mmol / 100 g.

[0026] By adopting the above technical scheme, the cation exchange capacity of sodium sericite is high, which can improve the degree of organic intercalation modification. The present invention adopts allyl cationic surfactant for intercalation modification, which can improve the interaction between the modified sericite and the PE substrate molecules, improve the dispersibility of sericite and enhance the reinforcing effect of sericite on the material. Maleic anhydride is also added in the modification process. The introduction of polar functional groups can improve the interfacial interaction between sericite and polycaprolactam, so that the sericite flake monomers can be evenly dispersed in the blending system. In this way, the well-dispersed sericite flake monomers can overlap each other inside the matrix to form a three-dimensional network structure, thereby improving the overall heat resistance of the material.

[0027] After being modified by organic intercalation, the sericite flake monomers can effectively block the transfer of heat, forming a barrier effect, and restricting the movement of the molecular chains of the polymer matrix, reducing the transfer of heat inside the material, and improving the heat resistance of the material.

[0028] Moreover, during the longitudinal stretching of the material, the stretching effect promotes the breakage of the molecular chains of the PE matrix, making it difficult to form crystal nuclei, reducing the crystallization efficiency and narrowing the crystallization peak width, thereby affecting the heat resistance of the material. After the addition of organic intercalated modified sericite flake monomers, the breakage rate of the molecular chains of the PE matrix is ​​significantly reduced, and the molecular chains can form stable crystal nuclei and promote crystal nucleus growth, thereby increasing crystallinity. At this time, further longitudinal stretching can help improve the performance of the PE film and improve the heat resistance of the material.

[0029] Preferably, the organic intercalation modified sericite flake monomer is also grafted with a polystyrene chain segment.

[0030] By adopting the above technical solution, the surface of the organic intercalation modified sericite flake monomer is also grafted with a polystyrene chain segment. The introduction of the polystyrene chain segment can better improve the affinity between the sericite flake monomer and the polymer molecular chain, so that the PE matrix molecular chain is easily adsorbed on the surface of the sericite flake monomer to form a crystal nucleus, promote the heterogeneous nucleation of PE, and reduce the adverse effects of longitudinal stretching on the PE material. At the same time, the introduction of the benzene ring rigid group in the polystyrene chain segment can also improve the overall thermal stability and better improve the heat resistance of the MDOPE film.

[0031] Preferably, the organic intercalation modified sericite flake monomer is prepared according to the following method:

[0032] S101. dispersing sodium sericite in a solvent, adding an allyl cationic surfactant and maleic anhydride, reacting at 80-100° C. for 4-5 hours, centrifuging, washing, drying, and finally ball-milling to obtain sericite flake monomers;

[0033] S102. Add a dispersant and a buffer to water, raise the temperature to 50-60°C, add the sericite flake monomer, initiator and styrene obtained in step S1, stir and disperse for 15-20 minutes, then raise the temperature to 80-90°C, react for 3-4 hours, filter, wash and dry to obtain an organic intercalation modified sericite flake monomer.

[0034] Preferably, the mass ratio of sericite flake monomer to styrene is 1:(10-12).

[0035] Preferably, the solvent in step S101 includes one or more of N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone.

[0036] Preferably, the ball-to-material ratio in the ball milling process is (5-10):1.

[0037] Preferably, the dispersant includes one or more combinations of polyvinyl alcohol, polyethylene glycol, polyvinyl pyrrolidone, and polyoxyethylene octylphenyl ether.

[0038] Preferably, the buffer comprises a combination of one or more of sodium bicarbonate, sodium acetate and magnesium carbonate.

[0039] Preferably, the initiator includes a combination of one or more of dibenzoyl peroxide, azobisisobutyronitrile, benzoyl peroxide, and potassium persulfate.

[0040] By adopting the above technical solution, maleic anhydride reacts with the silanol group on the surface of sericite, so that maleic anhydride can be smoothly grafted on the surface of sericite, improving the compatibility with polycaprolactam. After organic intercalation modification, it is ball-milled to form sericite flake monomers, reduce the particle size of sericite, and orient along the film direction during MDO stretching without changing the structure of sericite. The surface of the sericite flake monomer after intercalation modification with an allyl cationic surfactant contains double bond groups. Styrene can be grafted and copolymerized on the surface of sericite with double bonds as the reaction active center to form polystyrene segments, improve the thermal stability of the material, and further obtain the organic intercalation modified sericite flake monomers can improve the overall heat resistance.

[0041] Preferably, the MDOPE membrane is prepared according to the following method:

[0042] S201. The polycaprolactam is dried at 80 to 90 ° C;

[0043] S202. Weigh the corresponding mass fractions of polyethylene, dried polycaprolactam, compatibilizer, antioxidant and organic intercalation modified sericite flake monomer, mix them evenly, and then obtain a pretreated sheet by melt plasticization and extrusion casting;

[0044] S203. After preheating the pretreated sheet, longitudinally stretch the film at 130-150° C., and then shape and cool the film to obtain an MDOPE film.

[0045] Preferably, the melt plasticizing temperature in step S202 is 180-260°C.

[0046] Preferably, in step S203, the preheating temperature is 90-110°C; and the shaping temperature is 140-150°C.

[0047] Beneficial effects of the present invention:

[0048] 1. The raw materials of the MDOPE film of the present invention are polyethylene and polycaprolactam blended, and polycaprolactam can improve the overall heat resistance of the material.

[0049] 2. The MDOPE film of the present invention also contains organic intercalation modified sericite flake monomers, which can block the transfer of heat, improve the crystallization ability of the matrix, and are not adversely affected by the longitudinal stretching effect. The nano-scale sericite flake monomers can be oriented along the film direction during the MDO stretching process without changing their own structure, and will not affect the improvement effect on the material. After grafting with maleic anhydride, the compatibility of the sericite flake monomers in the material can be improved, and the three-dimensional network structure formed by overlapping each other can improve the overall heat resistance of the material. Furthermore, polystyrene chain segments are also grafted on the surface of the organic intercalation modified sericite flake monomers, which can improve the affinity with the polymer molecular chain, facilitate the adsorption of PE molecular chains on the sericite surface for heterogeneous nucleation, and improve the thermal stability of the material. DETAILED DESCRIPTION

[0050] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0051] Preparation Example

[0052] Preparation Example 1: An organic intercalation modified sericite flake monomer is prepared according to the following method:

[0053] Preparation of sodium sericite: 10 g of sericite raw material (average particle size of 800 mesh) was calcined at 800°C for 1 h, then added to 500 mL of 1.5 g / 100 mL nitric acid solution, the temperature was raised to 90°C, stirred for reaction for 4 h, and then filtered and dried to obtain acidified sericite; the acidified sericite was added to 250 mL of 4 g / 100 mL sodium chloride solution, the temperature was raised to 95°C, stirred for reaction for 15 h, and finally filtered, washed and dried to obtain sodium sericite.

[0054] 10 g of sodium sericite was dispersed in 500 mL of N,N-dimethylformamide, 15 g of hexadecyl dimethyl allyl ammonium chloride and 5 g of maleic anhydride were added, and the mixture was reacted at 90 °C for 5 h, followed by centrifugation, washing, drying, and ball milling to obtain organic intercalated modified sericite flake monomers, wherein the ball-to-material ratio was 10:1.

[0055] Preparation Example 2, an organic intercalation modified sericite flake monomer, is different from Preparation Example 1 only in that the added amount of hexadecyl dimethyl allyl ammonium chloride is 12 g and the added amount of maleic anhydride is 6 g.

[0056] Preparation Example 3, an organic intercalation modified sericite flake monomer, is different from Preparation Example 1 only in that the added amount of hexadecyl dimethyl allyl ammonium chloride is 18 g and the added amount of maleic anhydride is 4 g.

[0057] Preparation Example 4, an organic intercalation modified sericite flake monomer, is different from Preparation Example 1 only in that the amount of maleic anhydride added is 2 g.

[0058] Preparation Example 5, an organic intercalation modified sericite flake monomer, is different from Preparation Example 1 only in that the amount of maleic anhydride added is 8 g.

[0059] Preparation Example 6, an organic intercalation modified sericite flake monomer, is different from Preparation Example 1 only in that maleic anhydride is not added.

[0060] Preparation Example 7, an organic intercalation modified sericite flake monomer, is different from Preparation Example 1 only in that an equal amount of hexadecyltrimethylammonium bromide is used to replace hexadecyldimethylallylammonium chloride.

[0061] Preparation Example 8, an organic intercalation modified sericite flake monomer, is different from Preparation Example 1 only in that the organic intercalation modified sericite flake monomer is directly obtained after intercalation modification without ball milling treatment.

[0062] Preparation Example 9, an organic intercalation modified sericite flake monomer, prepared according to the following method:

[0063] Preparation of sodium sericite: 10 g of sericite raw material (average particle size of 800 mesh) was calcined at 800°C for 1 h, then added to 500 mL of 1.5 g / 100 mL nitric acid solution, the temperature was raised to 90°C, stirred for reaction for 4 h, and then filtered and dried to obtain acidified sericite; the acidified sericite was added to 250 mL of 4 g / 100 mL sodium chloride solution, the temperature was raised to 95°C, stirred for reaction for 15 h, and finally filtered, washed and dried to obtain sodium sericite.

[0064] 10 g of sodium sericite was dispersed in 500 mL of N,N-dimethylformamide, 15 g of hexadecyl dimethyl allyl ammonium chloride and 5 g of maleic anhydride were added, and the mixture was reacted at 90 °C for 5 h, followed by centrifugation, washing, drying, and ball milling to obtain sericite flake monomers, wherein the ball-to-material ratio was 10:1.

[0065] 1.5 g of polyvinyl alcohol (polyvinyl alcohol type 1799) and 7.5 g of sodium bicarbonate were added to 500 mL of water, the temperature was raised to 60°C, 10 g of the above-obtained sericite flake monomer, 2.5 g of dibenzoyl peroxide and 110 g of styrene were added, and after stirring and dispersing for 15 minutes, the temperature was raised to 90°C, and after reacting for 4 hours, the organic intercalation modified sericite flake monomer was obtained by filtration, washing and drying.

[0066] Preparation Example 10, an organic intercalation modified sericite flake monomer, is different from Preparation Example 9 only in that the amount of styrene added is 100 g.

[0067] Preparation Example 11, an organic intercalation modified sericite flake monomer, is different from Preparation Example 9 only in that the amount of styrene added is 120 g.

[0068] Example

[0069] Example 1: A MDOPE film with high heat resistance is prepared according to the following method:

[0070] Polycaprolactam (density 1.13 g / cm 3 ) and dried at 80° C. for 2 h; weighing 8 kg of polyethylene, 1.2 kg of dried polycaprolactam, 0.4 kg of high-density polyethylene grafted maleic anhydride (model W1 H), 0.1 kg of antioxidant 1010, 0.1 kg of antioxidant 168 and 0.8 kg of the organic intercalation modified sericite flake monomer prepared in Preparation Example 1, mixing them evenly, and then melting and plasticizing and extruding the cast sheet to obtain a pretreated sheet;

[0071] The polyethylene is a medium-density polyethylene (density 0.934 g / cm 3 , melt index is 12.5g / 10min) and high-density polyethylene (density is 0.95g / cm 3 , a mixture with a melt index of 10 g / 10 min).

[0072] The temperature of the melt plasticization section is 245°C.

[0073] The pretreated sheet was preheated to 90°C and then longitudinally stretched at 145°C. The film was then shaped at a temperature of 140°C and cooled to obtain an MDOPE film.

[0074] Example 2 and Example 3 are MDOPE films with high heat resistance. The difference from Example 1 is that the ratio of the raw materials is adjusted, as shown in Table 1:

[0075] Table 1 Formula table of Example 1 to Example 3

[0076]

[0077]

[0078] Example 4, a MDOPE film with high heat resistance, is different from Example 1 only in that the polyethylene is a mixture of medium-density polyethylene and high-density polyethylene in a mass ratio of 60:40; the organic intercalated modified sericite flake monomer prepared in Preparation Example 1 is replaced by an equal amount of the organic intercalated modified sericite flake monomer prepared in Preparation Example 2.

[0079] Example 5, a MDOPE film with high heat resistance, the only difference from Example 1 is that the polyethylene is a mixture of medium-density polyethylene and high-density polyethylene in a mass ratio of 80:20; the organic intercalated modified sericite flake monomer prepared in Preparation Example 1 is replaced by an equal amount of the organic intercalated modified sericite flake monomer prepared in Preparation Example 3.

[0080] Example 6, a MDOPE film with high heat resistance, is different from Example 1 only in that the organic intercalation modified sericite flake monomer prepared in Preparation Example 1 is replaced by an equal amount of the organic intercalation modified sericite flake monomer prepared in Preparation Example 4.

[0081] Example 7, a MDOPE film with high heat resistance, is different from Example 1 only in that the organic intercalation modified sericite flake monomer prepared in Preparation Example 1 is replaced by an equal amount of the organic intercalation modified sericite flake monomer prepared in Preparation Example 5.

[0082] Example 8, a MDOPE film with high heat resistance, is different from Example 1 only in that the organic intercalation modified sericite flake monomer prepared in Preparation Example 1 is replaced by an equal amount of the organic intercalation modified sericite flake monomer prepared in Preparation Example 7.

[0083] Example 9, a MDOPE film with high heat resistance, is different from Example 1 only in that the organic intercalation modified sericite flake monomer prepared in Preparation Example 1 is replaced by an equal amount of the organic intercalation modified sericite flake monomer prepared in Preparation Example 9.

[0084] Example 10, a MDOPE film with high heat resistance, is different from Example 1 only in that the organic intercalation modified sericite flake monomer prepared in Preparation Example 1 is replaced by an equal amount of the organic intercalation modified sericite flake monomer prepared in Preparation Example 10.

[0085] Example 11, a MDOPE film with high heat resistance, is different from Example 1 only in that the organic intercalation modified sericite flake monomer prepared in Preparation Example 1 is replaced by an equal amount of the organic intercalation modified sericite flake monomer prepared in Preparation Example 11.

[0086] Example 12, a MDOPE film with high heat resistance, is different from Example 1 only in that an equal amount of medium-density polyethylene is used to replace the polyethylene obtained by mixing medium-density polyethylene and high-density polyethylene in a mass ratio of 70:30.

[0087] Comparative Example

[0088] Comparative Example 1 is a MDOPE film with high heat resistance, which is different from Example 1 only in that the organic intercalation modified sericite flake monomer prepared in Preparation Example 1 is replaced by an equal amount of the organic intercalation modified sericite flake monomer prepared in Preparation Example 6.

[0089] Comparative Example 2 is a MDOPE film with high heat resistance, which is different from Example 1 only in that the organic intercalation modified sericite flake monomer prepared in Preparation Example 1 is replaced by an equal amount of the organic intercalation modified sericite flake monomer prepared in Preparation Example 8.

[0090] Comparative Example 3, a MDOPE film with high heat resistance, is different from Example 1 only in that the organic intercalation modified sericite flake monomer prepared in Preparation Example 1 is replaced by an equal amount of sericite raw material (average particle size of 800 mesh).

[0091] Comparative Example 4 is a MDOPE film with high heat resistance, which is different from Example 1 only in that no organic intercalation modified sericite flake monomer is added.

[0092] Comparative Example 5 is a MDOPE film with high heat resistance, which is different from Example 1 only in that polycaprolactam is not added.

[0093] Performance testing

[0094] Heat resistance test: According to the relevant records in GB / T 34848-2017 "Test method for shrinkage performance of heat shrinkable films", the heat shrinkage rate of the MDOPE film obtained in the examples and comparative examples was tested, wherein the test temperature was 120°C and the test time was 20 min.

[0095] The test results are shown in Table 2:

[0096] Table 2 Performance test results

[0097]

[0098] According to Table 2, in combination with Example 1 and Example 2 to Example 5, it can be seen that the heat shrinkage of Example 2 to Example 5 has no significant change compared with Example 1. Compared with Example 1, only the raw materials and their raw material ratios are adjusted within the required range in Example 2 to Example 5, which has little effect on the performance of the obtained MDOPE film.

[0099] Combining Example 1, Example 6, Example 7 and Comparative Example 1, it can be seen that the heat shrinkage rates of Example 6 and Example 7 are increased compared with Example 1, and the increase in Comparative Example 1 is obvious. Specifically, in Example 6, the amount of maleic anhydride grafted is reduced, the interface bonding force between the sericite flake monomer and polycaprolactam decreases, the dispersibility of the sericite flake monomer decreases, and the overall heat resistance decreases. In Comparative Example 1, no maleic anhydride grafted modified sericite flake monomer is added, and the performance decreases more significantly. In Example 7, the amount of maleic anhydride is increased, and the increased polarity is not conducive to the compatibility between the sericite flake monomer and the PE substrate, and the dispersibility decreases.

[0100] Combining Example 1 and Example 8, it can be seen that the heat shrinkage rate of Example 8 is increased compared with Example 1. In Example 8, a surfactant without double bonds is used to intercalate and modify sericite, and the compatibility with the PE substrate is reduced. The dispersibility of sericite is reduced during the film preparation process, and the effect of improving the overall thermal stability of the material is reduced.

[0101] Combining Example 1, Example 9 to Example 11, it can be seen that the heat shrinkage rate of Example 9 is lower than that of Example 1. The surface of the organic intercalation modified sericite flake monomer used in Example 9 is also grafted with polystyrene segments. While improving the affinity between the organic intercalation modified sericite flake monomer and the PE substrate, it can also promote the adsorption of PE molecular chains on the surface of the organic intercalation modified sericite flake monomer, perform heterogeneous nucleation, increase the growth rate of crystal nuclei, further increase the crystallization area inside the film, improve the rigidity of the material, reduce the influence of the stretching effect and improve the overall heat resistance. Example 10 and Example 11 are based on Example 9, and the raw material ratio is adjusted within the required range, which has little effect on the material properties.

[0102] Combining Example 1 and Example 12, it can be seen that the heat shrinkage rate of Example 12 is increased compared with Example 1. In Example 12, medium-density and high-density polyethylene blending is not adopted, and the overall density of the raw material decreases. After longitudinal oriented stretching, the molecular structure of the material changes, reducing the heat resistance of the material.

[0103] In combination with Example 1 and Comparative Examples 2 to 4, it can be seen that the heat shrinkage rates of Comparative Examples 2 to 4 are significantly increased compared to Example 1. Specifically, in Comparative Example 2, the organic intercalation-modified sericite was not ball-milled, and the sericite did not form a flake monomer form, but existed in a layered form. The increase in particle size will easily lead to the destruction of the crystal morphology of the organic intercalation-modified sericite during the longitudinal stretching process, thereby affecting the improvement of the heat resistance of the material. In Comparative Example 3, the sericite was not intercalated and modified, and the compatibility between the sericite and the PE matrix was significantly reduced. The uneven dispersion of sericite is not conducive to the improvement of material performance, but will cause internal defects in the material and reduce the material performance. In Comparative Example 4, no organic intercalation-modified sericite flake monomer was added, and the improvement of the thermal stability of the material and the improvement of the crystallinity of the material were lacking, and the heat resistance of the material was significantly reduced.

[0104] Combining Example 1 and Comparative Example 5, it can be seen that the heat shrinkage rate of Comparative Example 5 is increased compared with that of Example 1. In Comparative Example 5, polycaprolactam and polyethylene are not blended. On the one hand, the polycaprolactam itself lacks the enhancement of the thermal stability of the material and the increase of the raw material density. On the other hand, the organic intercalation modified sericite flake monomer cannot cooperate with polycaprolactam and polyethylene to form a three-dimensional network structure, thereby reducing the molecular chain density and the heat resistance of the film.

[0105] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0106] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A MDOPE film with high heat resistance, It is characterized in that The MDOPE film comprises the following raw materials in parts by weight: 75-85 parts of polyethylene; 10-15 parts of polycaprolactam; 3-5 parts of compatibilizer; 1 to 3 parts of antioxidant; 6 to 10 parts of organic intercalation modified sericite flake monomer; Maleic anhydride is also grafted on the surface of the organic intercalation modified sericite flake monomer.

2. The MDOPE film having high heat resistance according to claim 1, It is characterized in that The polyethylene is medium-density polyethylene and high-density polyethylene in a mass ratio of (60-80):(20-40).

3. The MDOPE film having high heat resistance according to claim 1, It is characterized in that The raw materials of the organic intercalation modified sericite flake monomer include sodium sericite, allyl cationic surfactant and maleic anhydride in a mass ratio of 1: (1.2-1.8): (0.4-0.6).

4. The MDOPE film having high heat resistance according to claim 3, It is characterized in that The allyl cationic surfactant includes one or more of hexadecyl dimethyl allyl ammonium chloride, dodecyl dimethyl allyl ammonium chloride, octadecyl dimethyl allyl ammonium chloride, allyl trimethyl ammonium bromide, and diallyl dimethyl ammonium chloride.

5. The MDOPE film having high heat resistance according to claim 3, It is characterized in that The organic intercalation modified sericite flake monomer is also grafted with a polystyrene chain segment.

6. The MDOPE film having high heat resistance according to claim 5, It is characterized in that The organic intercalation modified sericite flake monomer is prepared according to the following method: S101. dispersing sodium sericite in a solvent, adding an allyl cationic surfactant and maleic anhydride, reacting at 80-100° C. for 4-5 hours, centrifuging, washing, drying, and finally ball-milling to obtain sericite flake monomers; S102. Add a dispersant and a buffer to water, raise the temperature to 50-60°C, add the sericite flake monomer, initiator and styrene obtained in step S1, stir and disperse for 15-20 minutes, then raise the temperature to 80-90°C, react for 3-4 hours, filter, wash and dry to obtain an organic intercalation modified sericite flake monomer.

7. The MDOPE film having high heat resistance according to claim 6, It is characterized in that The mass ratio of the sericite flake monomer to styrene is 1:(10-12).

8. The MDOPE film having high heat resistance according to claim 1, It is characterized in that The compatibilizer includes one or a combination of maleic anhydride grafted compatibilizer and acrylic acid type compatibilizer.

9. The MDOPE film having high heat resistance according to claim 1, It is characterized in that The antioxidant is one or a combination of two of a phenolic antioxidant and a phosphite antioxidant.

10. The MDOPE film having high heat resistance according to claim 1, It is characterized in that The MDOPE film is prepared according to the following method: S201. The polycaprolactam is dried at 80 to 90 ° C; S202. Weigh the corresponding mass fractions of polyethylene, dried polycaprolactam, compatibilizer, antioxidant and organic intercalation modified sericite flake monomer, mix them evenly, and then obtain a pretreated sheet by melt plasticization and extrusion casting; S203. After preheating the pretreated sheet, longitudinally stretch the film at 130-150° C., and then shape and cool the film to obtain an MDOPE film.