Automobile sound insulation sealing rubber prepared from reclaimed rubber and preparation method of automobile sound insulation sealing rubber
By using butyl recycled glue and modification additives in automotive sealing strip materials, combined with grafting technology of modified mesoporous silica and glass fiber, the performance degradation of sealing strips under high temperature and oxygen stress is solved, and the performance of sealing strips is achieved. Excellent mechanical, sound absorption and aging resistance extend the service life of the seal.
Patent Information
- Application Number
- CN202411399672.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing automotive sealing strip materials have deteriorated performance under high temperature and oxygen stress, which is flammable and has insufficient aging resistance, resulting in faster loss of seals and cannot meet the needs of long-term use.
Use butyl recycled rubber, ethylene propylene ternary rubber and polyvinyl chloride as substrates, and add modified additives to prepare modified mesoporous silica and modified glass fibers through chemical reaction and grafting technology to form flame retardant and Components with aging resistance and mixed with adjuvants such as tackifying resins and zinc oxide, and vulcanizing treatment to improve mechanical properties and sound absorption and sound insulation properties.
Seal rubber with excellent mechanical properties, sound absorption and sound insulation properties, high temperature aging resistance and flame retardant properties were prepared, which extends the service life of the seal and reduces losses.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rubber materials, and in particular relates to an automobile sound insulation sealing rubber prepared by utilizing recycled rubber and a preparation method thereof. Background Art
[0002] Automobile sealing strips are a type of strip-shaped sealing product made of rubber or plastic, which is widely used in car doors, windows, trunks, engine compartments, etc. Automobile sealing strips generally use EPDM rubber or polyvinyl chloride as raw materials. Among them, EPDM rubber has excellent mechanical properties and good processing properties, so it occupies more than 80% of the automobile sealing strip market.
[0003] With the development of automobile industry and transportation industry, the demand for tires is increasing day by day, which brings up the question of how to utilize waste tires. The main way to utilize waste tires is to process them into recycled rubber. Butyl recycled rubber is an important product category of recycled rubber. It uses butyl inner tube as raw material and adopts advanced decomposition process to filter and refine after desulfurization. It has the characteristics of good strength, high fineness, strong air tightness, rich elasticity, etc. It can be blended with a variety of rubbers. Adding butyl recycled rubber to automobile sound insulation sealant can improve the air tightness of the rubber and reduce the cost of the rubber.
[0004] Noise is a common environmental pollution. Long-term exposure to a high-noise environment will have a great impact on people's lives. Rubber particles are flexible materials with a certain degree of elasticity. They can effectively absorb the vibration of sound waves, thereby reducing sound pressure. However, rubber materials are flammable, and the increase in the amount of such flexible materials will greatly reduce the strength of the substrate. In addition, external environmental stresses such as high temperature and oxygen will inevitably cause the physical and mechanical properties and aging resistance of rubber sealing materials to decline significantly, resulting in the degradation of product performance and making it unable to meet the needs of normal operation, accelerating the loss of seals and high-temperature seal failure. Summary of the invention
[0005] In order to solve the deficiencies mentioned in the above background technology, the purpose of the present invention is to provide an automotive sound insulation sealing rubber prepared by recycled rubber and a preparation method thereof, taking butyl recycled rubber, EPDM rubber and polyvinyl chloride as the base material, adding modified additives to give the rubber material excellent mechanical properties, sound absorption and sound insulation properties, high temperature aging resistance and flame retardant properties.
[0006] The purpose of the present invention can be achieved by the following technical solutions: A car sound insulation sealing rubber prepared by using recycled rubber, comprising the following components in parts by weight: 40-60 parts of butyl recycled rubber, 10-20 parts of EPDM rubber, 5-10 parts of polyvinyl chloride, 5-15 parts of modified additives, 2-5 parts of tackifying resin, 2-5 parts of zinc oxide, 1-2 parts of lubricant, 0.5-2.5 parts of sulfur, and 0.1-1 parts of accelerator; The modified additive is prepared by grafting modified mesoporous silica and modified glass fiber with component two through chemical reaction, wherein the modified mesoporous silica is prepared by grafting with 1,5-naphthalene diamine after aldehyde group modification with 3-aminopropyl triethoxysilane and glutaraldehyde; the modified glass fiber is prepared by amino modification with a silane coupling agent; and component two is prepared by grafting with maleic anhydride after phenylphosphoryl dichloride and antioxidant N-(4-anilinophenyl) maleimide.
[0007] Preferably, the lubricant is a combination of one or more of stearic acid, polyethylene wax, and oxidized polyethylene wax; and the accelerator is a mixture of one or more of accelerator TMTD, accelerator DM, accelerator DTDM, and accelerator NS.
[0008] Preferably, the preparation method of the modified additive comprises the following steps: A. Phenylphosphoryl dichloride and N-(4-anilinophenyl)maleimide are placed in a reactor, tetrahydrofuran solvent is added and stirred evenly, then solid sodium hydroxide is added, and the mixture is condensed and refluxed for 5 to 7 hours. After the reaction is completed, the mixture is rotary evaporated and dried, and the obtained solid product is dissolved in methanol, filtered, rotary evaporated, and dried to prepare component 1; B. Component 1 and maleic anhydride are dissolved in cyclohexanone, nitrogen is passed through the reaction, the mixture is stirred at 45-60° C., azobisisobutyronitrile is added, the mixture is reacted at 80-95° C. for 2-4 hours, and after the reaction is completed, the mixture is filtered, washed, and dried to prepare component 2; C. Take component 2 and cyclohexanone and dissolve them in a reactor to obtain a polymer solution, then add modified mesoporous silica and modified glass fiber and disperse them by ultrasonic, place them at 60-85°C and stir to react for 3-5 hours. After the reaction is completed, filter, wash and dry to obtain a modified additive.
[0009] Preferably, in step A, the molar ratio of phenylphosphoryl dichloride to N-(4-anilinophenyl)maleimide is 1:2-2.5.
[0010] Preferably, in step B, the molar ratio of component 1, maleic anhydride and azobisisobutyronitrile is 1:2-2.7:0.03-0.07.
[0011] Preferably, the preparation method of modified mesoporous silica in step C comprises the following steps: (1) P123 was dissolved in a mixed solution of deionized water and hydrochloric acid, tetraethyl orthosilicate was added, and the mixture was stirred at 40-50°C for 20-24 hours. After the reaction was completed, the mixture was moved to an autoclave and kept at 95-105°C for 20-24 hours. After the reaction was completed, the mixture was centrifuged, washed, and dried, and the obtained product was placed in a muffle furnace and calcined at 450-550°C for 3-5 hours to prepare mesoporous silica. (2) adding anhydrous toluene and 3-aminopropyltriethoxysilane to mesoporous silica, and subjecting the mixture to reflux reaction at 100-120°C for 42-48 hours. After the reaction is completed, the mixture is centrifuged, washed, and dried. The obtained product is added with glutaraldehyde solution, and subjecting the mixture to stirring reaction at 30-40°C for 3-5 hours. After the reaction is completed, the mixture is centrifuged, washed, and dried to prepare aldehyde-modified mesoporous silica. (3) Take aldehyde-modified mesoporous silica and 1,5-naphthalenediamine in a reactor, add ethanol solvent to disperse them evenly by ultrasonication, and place them under reflux reaction at 55-70°C for 4-7 hours. After the reaction is completed, filter, wash and dry to prepare modified mesoporous silica.
[0012] Preferably, the concentration of the glutaraldehyde solution in step (2) is 5-10%, and the addition ratio of the mesoporous silica, 3-aminopropyltriethoxysilane and glutaraldehyde solution is 1 g: 4-6 mL: 45-70 mL.
[0013] Preferably, the method for preparing the modified glass fiber in step C comprises the following steps: ① The glass fiber is placed in an acetone solution for ultrasonic treatment and soaking, and then dried and then soaked in a mixed solution of concentrated sulfuric acid and hydrogen peroxide to obtain pretreated glass fiber after drying; ② The pretreated glass fiber is immersed in a mixed solution of 3-aminopropyltriethoxysilane and toluene, placed under condensation reflux at 90-120° C. for 8-12 hours, and then washed and dried to prepare the modified glass fiber.
[0014] The method for preparing the automobile sound insulation sealing rubber prepared by using the reclaimed rubber as described above comprises the following steps: adding parts by weight of butyl reclaimed rubber, EPDM rubber and polyvinyl chloride into an open mill for plasticizing, adding parts by weight of a modifying additive, a tackifying resin, zinc oxide and a lubricant for uniform mixing after the plasticizing is uniform, and finally adding parts by weight of sulfur and an accelerator for uniform mixing and vulcanizing at 120-160° C. for 5-10 minutes to prepare the automobile sound insulation sealing rubber.
[0015] Beneficial effects of the present invention: The present invention uses butyl reclaimed rubber, EPDM rubber and polyvinyl chloride as base materials, and adds modifying additives, tackifying resins, zinc oxide and other additives to prepare sealing rubber with excellent mechanical properties, sound absorption and sound insulation properties, high temperature aging resistance and flame retardant properties. The present invention uses the chlorine atom in the structure of phenylphosphoryl dichloride and the -NH group in the structure of antioxidant N-(4-anilinophenyl) maleimide to undergo substitution reaction to prepare component one with flame retardant and aging resistance properties, and then copolymerizes component one and maleic anhydride under the action of azobisisobutyronitrile to prepare component two, and grafts the amino groups in the modified mesoporous silica and modified glass fiber structures with the maleic anhydride groups in the structure of component two to form a strong chemical bond, thereby preparing a modified additive.
[0016] The modified mesoporous silica is prepared by using 3-aminopropyltriethoxysilane and glutaraldehyde to modify the mesoporous silica with aldehyde groups, and then reacting the aldehyde groups with one-terminal amino group in the 1,5-naphthalenediamine structure. The pore structure of the mesoporous silica will hinder the propagation of sound waves, and the sound waves will be reflected on its surface and multiple reflections will occur in its cavity, thereby attenuating the sound energy and improving the sound insulation performance. 1,5-naphthalenediamine can achieve a synergistic flame retardant effect with phenylphosphinoyl dichloride, and can form a protective layer at high temperatures to prevent further transfer of oxygen and heat. The modified glass fiber is amino-modified with 3-aminopropyltriethoxysilane. The glass fiber has the properties of high strength, high insulation, corrosion resistance and high temperature resistance, and has a loose structure, so that air can flow between the structures, and has certain sound absorption characteristics. Grafting modified mesoporous silica and modified glass fiber to component two is beneficial to the dispersion of the filler and enables its performance to be effectively exerted. The added modified additives can give the material excellent mechanical properties and sound absorption and sound insulation effects, while also giving it excellent high temperature aging resistance and flame retardant properties. DETAILED DESCRIPTION
[0017] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0018] In the embodiments and comparative examples of the present invention, the butyl reclaimed rubber is produced by Hebei Hongyun Reclaimed Rubber Company; the polyvinyl chloride is produced by Sinopec Qingdao Refining and Chemical Co., Ltd.; and the tackifying resin is produced by Qingdao Sailun Tire Co., Ltd.
[0019] Example 1 A method for preparing modified mesoporous silica comprises the following steps: (1) 6 g of P123 was dissolved in a mixed solution of 170 mL of deionized water and 20 mL of 37% hydrochloric acid, 15 mL of tetraethyl orthosilicate was added, and the mixture was stirred at 45 °C for 24 h. After the reaction was completed, the mixture was moved to an autoclave and kept at 100 °C for 24 h. After the reaction was completed, the mixture was centrifuged, washed, and dried. The obtained product was placed in a muffle furnace and calcined at 500 °C for 4 h to prepare mesoporous silica. (2) 1 g of mesoporous silica was added with 25 mL of anhydrous toluene and 4 mL of 3-aminopropyltriethoxysilane, and the mixture was refluxed at 115°C for 42 h. After the reaction was completed, the mixture was centrifuged, washed, and dried. The obtained product was added with 50 mL of 7% glutaraldehyde solution, and the mixture was stirred at 40°C for 5 h. After the reaction was completed, the mixture was centrifuged, washed, and dried to prepare aldehyde-modified mesoporous silica. (3) 1.2 g of aldehyde-modified mesoporous silica and 1.58 g of 1,5-naphthalenediamine were placed in a reactor, ethanol solvent was added for ultrasonic dispersion, and the mixture was refluxed at 65 °C for 7 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain modified mesoporous silica.
[0020] Embodiment 2 A method for preparing a modified glass fiber comprises the following steps: ① The glass fiber is placed in an acetone solution for ultrasonic treatment and soaking, and then after drying, it is soaked in a mixed solution of concentrated sulfuric acid and hydrogen peroxide in a volume ratio of 7:3, and after drying, the pretreated glass fiber is obtained; ② The pretreated glass fiber was immersed in a 10% 3-aminopropyltriethoxysilane toluene solution, placed under condensation reflux at 110° C. for 12 hours, and then washed and dried to prepare the modified glass fiber.
[0021] Example 3 A method for preparing a modified additive comprises the following steps: A. Take 1.95g of phenylphosphoryl dichloride and 5.81g of N-(4-anilinophenyl)maleimide in a reactor, add 100mL of tetrahydrofuran solvent and stir evenly, then add 0.9g of sodium hydroxide solid, condense and reflux for 6h, after the reaction is completed, rotary evaporate and dry, dissolve the obtained solid product with methanol, filter, rotary evaporate and dry to prepare component 1; B. 8.13 g of component 1 and 2.94 g of maleic anhydride were dissolved in 50 mL of cyclohexanone, nitrogen was passed through the reaction, and the mixture was stirred at 55 ° C. Then 0.062 g of azobisisobutyronitrile was added, and the mixture was reacted at 95 ° C for 4 h. After the reaction was completed, the mixture was filtered, washed, and dried to prepare component 2; C. Take 5.62g of component 2 and 75mL of cyclohexanone and dissolve them in a reactor to obtain a polymer solution, then add 1.5g of modified mesoporous silica prepared in Example 1 and 2g of modified glass fiber prepared in Example 2 and disperse them by ultrasonic, place at 75°C and stir to react for 5h. After the reaction is completed, filter, wash and dry to obtain a modified additive.
[0022] Example 4 A car sound insulation sealing rubber prepared by using reclaimed rubber comprises the following components in parts by weight: 42 parts of butyl reclaimed rubber, 10 parts of EPDM rubber, 5 parts of polyvinyl chloride, 5 parts of the modified additive prepared in Example 3, 2 parts of tackifying resin, 2 parts of zinc oxide, 1 part of lubricant stearic acid, 0.7 parts of sulfur, and 0.2 parts of accelerator DM.
[0023] The preparation method of the above-mentioned automobile sound insulation sealing rubber comprises the following steps: Parts by weight of butyl reclaimed rubber, EPDM rubber and polyvinyl chloride are added to an open mill for plasticizing. After plasticizing evenly, parts by weight of modifying additives, tackifying resin, zinc oxide and lubricant are added and mixed evenly. Finally, parts by weight of sulfur and accelerator are added and mixed evenly, and then vulcanized at 145° C. for 8 minutes to prepare automotive sound insulation sealing rubber.
[0024] Example 5 A car sound insulation sealing rubber prepared by using reclaimed rubber comprises the following components in parts by weight: 51 parts of butyl reclaimed rubber, 16 parts of EPDM rubber, 7 parts of polyvinyl chloride, 10 parts of the modified additive prepared in Example 3, 4 parts of tackifying resin, 3 parts of zinc oxide, 2 parts of lubricant polyethylene wax, 1 part of sulfur, and 0.5 parts of accelerator TMTD.
[0025] The preparation method of the above-mentioned automobile sound insulation sealing rubber is the same as that of Example 4.
[0026] Example 6 A car sound insulation sealing rubber prepared by using recycled rubber comprises the following components in parts by weight: 60 parts of butyl reclaimed rubber, 18 parts of EPDM rubber, 10 parts of polyvinyl chloride, 14 parts of the modified additive prepared in Example 3, 4 parts of tackifying resin, 4 parts of zinc oxide, 2 parts of lubricant oxidized polyethylene wax, 2 parts of sulfur, and 1 part of accelerator TMTD.
[0027] The preparation method of the above-mentioned automobile sound insulation sealing rubber is the same as that of Example 4.
[0028] Comparative Example 1 A method for preparing a modified additive comprises the following steps: A. Take 1.95g of phenylphosphoryl dichloride and 5.81g of N-(4-anilinophenyl)maleimide in a reactor, add 100mL of tetrahydrofuran solvent and stir evenly, then add 0.9g of sodium hydroxide solid, condense and reflux for 6h, after the reaction is completed, rotary evaporate and dry, dissolve the obtained solid product with methanol, filter, rotary evaporate and dry to prepare component 1; B. 8.13 g of component 1 and 2.94 g of maleic anhydride were dissolved in 50 mL of cyclohexanone, nitrogen was passed through the reaction, and the mixture was stirred at 55 ° C. Then 0.062 g of azobisisobutyronitrile was added, and the mixture was reacted at 95 ° C for 4 h. After the reaction was completed, the mixture was filtered, washed, and dried to prepare component 2; C. Take 5.62 g of component 2 and 75 mL of cyclohexanone and dissolve them in a reactor to obtain a polymer solution, then add 1.5 g of the modified mesoporous silica prepared in Example 1 and disperse it ultrasonically, place it at 75°C and stir to react for 5 hours. After the reaction is completed, filter, wash and dry to obtain a modified additive.
[0029] Comparative Example 2 A method for preparing a modified additive comprises the following steps: A. Take 1.95g of phenylphosphoryl dichloride and 5.81g of N-(4-anilinophenyl)maleimide in a reactor, add 100mL of tetrahydrofuran solvent and stir evenly, then add 0.9g of sodium hydroxide solid, condense and reflux for 6h, after the reaction is completed, rotary evaporate and dry, dissolve the obtained solid product with methanol, filter, rotary evaporate and dry to prepare component 1; B. 8.13 g of component 1 and 2.94 g of maleic anhydride were dissolved in 50 mL of cyclohexanone, nitrogen was passed through the reaction, and the mixture was stirred at 55 ° C. Then 0.062 g of azobisisobutyronitrile was added, and the mixture was reacted at 95 ° C for 4 h. After the reaction was completed, the mixture was filtered, washed, and dried to prepare component 2; C. Take 5.62g of component 2 and 75mL of cyclohexanone and dissolve them in a reactor to obtain a polymer solution, then add 2g of the modified glass fiber prepared in Example 2 and disperse it ultrasonically, place it at 75°C and stir to react for 5h. After the reaction is completed, filter, wash and dry to obtain a modified additive.
[0030] Comparative Example 3 An automobile sound insulation sealing rubber prepared by using recycled rubber comprises the following components in parts by weight: 60 parts of butyl reclaimed rubber, 18 parts of EPDM rubber, 10 parts of polyvinyl chloride, 14 parts of the modified additive prepared in Comparative Example 1, 4 parts of tackifying resin, 4 parts of zinc oxide, 2 parts of lubricant oxidized polyethylene wax, 2 parts of sulfur, and 1 part of accelerator TMTD.
[0031] The preparation method of the above-mentioned automobile sound insulation sealing rubber is the same as that of Example 4.
[0032] Comparative Example 4 An automobile sound insulation sealing rubber prepared by using reclaimed rubber comprises the following components in parts by weight: 60 parts of butyl reclaimed rubber, 18 parts of EPDM rubber, 10 parts of polyvinyl chloride, 14 parts of the modified additive prepared in Comparative Example 2, 4 parts of tackifying resin, 4 parts of zinc oxide, 2 parts of lubricant oxidized polyethylene wax, 2 parts of sulfur, and 1 part of accelerator TMTD.
[0033] The preparation method of the above-mentioned automobile sound insulation sealing rubber is the same as that of Example 4.
[0034] Comparative Example 5 An automobile sound insulation sealing rubber prepared by using recycled rubber comprises the following components in parts by weight: 60 parts of butyl reclaimed rubber, 18 parts of EPDM rubber, 10 parts of polyvinyl chloride, 6 parts of mesoporous silica prepared in Example 1, 8 parts of modified glass fiber prepared in Example 2, 4 parts of tackifying resin, 4 parts of zinc oxide, 2 parts of lubricant oxidized polyethylene wax, 2 parts of sulfur, and 1 part of accelerator TMTD.
[0035] The preparation method of the above-mentioned automobile sound insulation sealing rubber is the same as that of Example 4.
[0036] Comparative Example 6 An automobile sound insulation sealing rubber prepared by using recycled rubber comprises the following components in parts by weight: 60 parts of butyl reclaimed rubber, 18 parts of EPDM rubber, 10 parts of polyvinyl chloride, 6 parts of modified mesoporous silica prepared in Example 1, 8 parts of modified glass fiber prepared in Example 2, 4 parts of tackifying resin, 4 parts of zinc oxide, 2 parts of lubricant oxidized polyethylene wax, 2 parts of sulfur, and 1 part of accelerator TMTD.
[0037] The preparation method of the above-mentioned automobile sound insulation sealing rubber is the same as that of Example 4.
[0038] Performance Testing The sound insulation sealing rubber prepared in Examples 4-6 and Comparative Examples 3-6 was subjected to performance tests: the tensile performance was tested with reference to GB / T 528-2009; the Shore A hardness was tested using a durometer; the resilience was tested using an impact elasticity testing machine; the aging resistance was tested with reference to GB / T 3512-2014, and the aging conditions were 70°C×168h; the oxygen index was tested according to GB / T 2406.2-2009; the sound absorption coefficient and sound insulation were tested using an impedance tube, and the sound wave frequency range was 1000~6000Hz, and the data results are shown in Table 1.
[0039] Table 1 Test results of sample performance
[0040] It can be seen from the data in Table 1 that the rubber materials prepared in Examples 4-6 of the present invention have good sound absorption and sound insulation performance, high strength and toughness, and excellent aging resistance and flame retardant properties. The modified additive added in Comparative Example 3 does not contain a modified glass fiber component, and the modified additive added in Comparative Example 4 does not contain a modified mesoporous silica component. The mechanical properties, sound absorption coefficients, and sound insulation values of Comparative Examples 3-4 are lower than those of Examples 4-6, indicating that the addition of modified glass fibers and modified mesoporous silica can improve the mechanical properties and sound absorption and sound insulation properties of the materials. The oxygen index of Comparative Example 4 is slightly lower than that of Examples 4-6 because the 1,5-naphthalenediamine component is not introduced, resulting in its flame retardant properties. Reduced, in Comparative Example 5, the unmodified mesoporous silica and the modified glass fiber were simply mixed, and the measured mechanical properties and sound absorption and sound insulation properties were slightly lower than those of Examples 4-6, which may be due to the agglomeration of mesoporous silica causing its performance to be reduced. In Comparative Example 6, the modified mesoporous silica and the modified glass fiber were simply mixed, and the measured tensile strength change rate, elongation at break change rate and oxygen index were significantly changed compared with Examples 4-6. The reason is that due to the ungrafted component two, its flame retardant properties and aging resistance are significantly reduced.
[0041] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0042] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.
Claims
1. An automobile sound insulation sealing rubber prepared by using recycled rubber, characterized in that: The invention comprises the following components in parts by weight: 40-60 parts of butyl reclaimed rubber, 10-20 parts of EPDM rubber, 5-10 parts of polyvinyl chloride, 5-15 parts of modified additives, 2-5 parts of tackifying resin, 2-5 parts of zinc oxide, 1-2 parts of lubricant, 0.5-2.5 parts of sulfur and 0.1-1 parts of accelerator; The modified additive is prepared by grafting modified mesoporous silica and modified glass fiber with component two through chemical reaction, wherein the modified mesoporous silica is prepared by grafting with 1,5-naphthalene diamine after aldehyde group modification with 3-aminopropyl triethoxysilane and glutaraldehyde; the modified glass fiber is prepared by amino modification with a silane coupling agent; and component two is prepared by grafting with maleic anhydride after phenylphosphoryl dichloride and antioxidant N-(4-anilinophenyl) maleimide.
2. The automobile sound insulation sealing rubber prepared by using reclaimed rubber according to claim 1, characterized in that: The lubricant is a combination of one or more of stearic acid, polyethylene wax, and oxidized polyethylene wax; the accelerator is a mixture of one or more of accelerator TMTD, accelerator DM, accelerator DTDM, and accelerator NS.
3. The automobile sound insulation sealing rubber prepared by using reclaimed rubber according to claim 1, characterized in that: The preparation method of the modified additive comprises the following steps: A. Phenylphosphoryl dichloride and N-(4-anilinophenyl)maleimide are placed in a reactor, tetrahydrofuran solvent is added and stirred evenly, then solid sodium hydroxide is added, and the mixture is condensed and refluxed for 5 to 7 hours. After the reaction is completed, the mixture is rotary evaporated and dried, and the obtained solid product is dissolved in methanol, filtered, rotary evaporated, and dried to prepare component 1; B. Component 1 and maleic anhydride are dissolved in cyclohexanone, nitrogen is passed through the reaction, the mixture is stirred at 45-60° C., azobisisobutyronitrile is added, the mixture is reacted at 80-95° C. for 2-4 hours, and after the reaction is completed, the mixture is filtered, washed, and dried to prepare component 2; C. Take component 2 and cyclohexanone and dissolve them in a reactor to obtain a polymer solution, then add modified mesoporous silica and modified glass fiber and disperse them by ultrasonic, place them at 60-85°C and stir to react for 3-5 hours. After the reaction is completed, filter, wash and dry to obtain a modified additive.
4. The automobile sound insulation sealing rubber prepared by using reclaimed rubber according to claim 3, characterized in that: In the step A, the molar ratio of phenylphosphoryl dichloride to N-(4-anilinophenyl)maleimide is 1:2-2.
5.
5. The automobile sound insulation sealing rubber prepared by using reclaimed rubber according to claim 3, characterized in that: In the step B, the molar ratio of component 1, maleic anhydride and azobisisobutyronitrile is 1:2-2.7:0.03-0.
07.
6. The automobile sound insulation sealing rubber prepared by using reclaimed rubber according to claim 3, characterized in that: The preparation method of the modified mesoporous silica in step C comprises the following steps: (1) P123 was dissolved in a mixed solution of deionized water and hydrochloric acid, tetraethyl orthosilicate was added, and the mixture was stirred at 40-50°C for 20-24 hours. After the reaction was completed, the mixture was moved to an autoclave and kept at 95-105°C for 20-24 hours. After the reaction was completed, the mixture was centrifuged, washed, and dried, and the obtained product was placed in a muffle furnace and calcined at 450-550°C for 3-5 hours to prepare mesoporous silica. (2) adding anhydrous toluene and 3-aminopropyltriethoxysilane to mesoporous silica, and subjecting the mixture to reflux reaction at 100-120°C for 42-48 hours. After the reaction is completed, the mixture is centrifuged, washed, and dried. The obtained product is added with glutaraldehyde solution, and subjecting the mixture to stirring reaction at 30-40°C for 3-5 hours. After the reaction is completed, the mixture is centrifuged, washed, and dried to prepare aldehyde-modified mesoporous silica. (3) Take aldehyde-modified mesoporous silica and 1,5-naphthalenediamine in a reactor, add ethanol solvent to disperse them evenly by ultrasonication, and place them under reflux reaction at 55-70°C for 4-7 hours. After the reaction is completed, filter, wash and dry to prepare modified mesoporous silica.
7. The automobile sound insulation sealing rubber prepared by using reclaimed rubber according to claim 6, characterized in that: The concentration of the glutaraldehyde solution in step (2) is 5-10%, and the addition ratio of the mesoporous silica, 3-aminopropyltriethoxysilane and glutaraldehyde solution is 1 g: 4-6 mL: 45-70 mL.
8. The automobile sound insulation sealing rubber prepared by using reclaimed rubber according to claim 3, characterized in that: The preparation method of the modified glass fiber in step C comprises the following steps: ① The glass fiber is placed in an acetone solution for ultrasonic treatment and soaking, and then dried and then soaked in a mixed solution of concentrated sulfuric acid and hydrogen peroxide to obtain pretreated glass fiber after drying; ② The pretreated glass fiber is immersed in a mixed solution of 3-aminopropyltriethoxysilane and toluene, placed under condensation reflux at 90-120° C. for 8-12 hours, and then washed and dried to prepare the modified glass fiber.
9. A method for preparing automobile sound insulation sealing rubber using reclaimed rubber as claimed in any one of claims 1 to 8, characterized in that: The following steps are involved: Parts by weight of butyl reclaimed rubber, EPDM rubber and polyvinyl chloride are added to an open mill for plasticizing. After plasticizing evenly, parts by weight of modifying additives, tackifying resin, zinc oxide and lubricant are added and mixed evenly. Finally, parts by weight of sulfur and accelerator are added and mixed evenly, and then vulcanized at 120-160° C. for 5-10 minutes to prepare automotive sound insulation sealing rubber.
Citation Information
Cited By
Low-VOC (volatile organic compound) automobile sealing strip composite PVC (polyvinyl chloride) material and preparation method thereof
CN119241967A