Low-temperature-resistant tear-resistant plastic film and preparation method thereof

By using blending modification technology of ethylene fluoride, trifluoroethylene copolymer and maleic anhydride grafted polyolefin elastomer in the film, the tear resistance and flexibility of traditional films under low temperature environments are solved. The problem of this problem significantly improves tear resistance and low temperature resistance.

CN119060474AInactive Publication Date: 2024-12-03TAIZHOU HUAQIANSHU PLASTIC IND CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410950562.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional films have reduced tear resistance and reduced flexibility in low temperature environments, and cannot meet the material needs in aerospace, polar investigation, deep-sea exploration and other fields.

Method used

Using blending and modification technology, vinylidene fluoride homopolymer generated by monomer polymerization is used as the matrix material, maleic anhydride grafted polyolefin elastomer and nanomagnesium sulfate filler are introduced, and ultrasonic air is used. Chemical treatment and twin-screw extrusion casting make a film to improve the dispersion and compatibility of nanomagnesium sulfate and enhance the impact resistance of the film.

Benefits of technology

It significantly improves the tear strength and low temperature resistance of the film, improves the compatibility and dispersion of inorganic nanofillers and polyvinylidene fluoride, and enhances the impact resistance and ultraviolet resistance of the film.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a low-temperature-resistant tear-resistant plastic film and a preparation method thereof, and relates to the field of film materials. The low-temperature-resistant and tear-resistant film is prepared from the following components in percentage by mass: 50 to 80 parts of polyvinylidene fluoride, 20 to 40 parts of polymethyl methacrylate, 80 to 100 parts of polyoxyethylene (POE), 1 to 5 parts of maleic anhydride, 1 to 5 parts of inorganic nano filler, 1 to 3 parts of organic ultraviolet light absorber, 0.2 to 0.5 part of antioxidant, 0.1 to 0.5 part of peroxide, 0.1 to 0.5 part of cross-linking inhibitor and 1 to 2 parts of lubricant. The low-temperature-resistant and tear-resistant film prepared by the invention has the advantages of low temperature resistance, good tear resistance, strong impact resistance, ultraviolet resistance and long service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, in particular to a low-temperature resistant and tear-resistant plastic film and a preparation method thereof. Background Art

[0002] With the continuous advancement of science and technology, the demand for material applications in special environments is increasing. In extremely low temperature environments, traditional film materials often have problems such as hardening and brittleness, resulting in a significant decrease in their performance and being unable to meet the needs of practical applications. Especially in the fields of aerospace, polar exploration, deep-sea exploration, etc., higher requirements are placed on the low-temperature resistance of materials.

[0003] As an important functional material, film is widely used in packaging, protection, insulation and other fields. However, traditional films have obvious performance defects in low temperature environments, such as reduced tear strength and decreased flexibility, which seriously limit their application in special environments. Therefore, it is necessary to study a low temperature resistant and tear resistant film. Summary of the invention

[0004] The purpose of the present invention is to provide a low-temperature resistant and tear-resistant plastic film and a preparation method thereof to solve the problems existing in the prior art.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a low-temperature resistant and tear-resistant film, wherein the low-temperature resistant and tear-resistant film components include, in terms of mass percentage: 50 to 80 parts of polyvinylidene fluoride, 20 to 40 parts of polymethyl methacrylate, 1 to 5 parts of maleic anhydride grafted polyolefin elastomer, 1 to 5 parts of inorganic nanofiller, 1 to 3 parts of organic ultraviolet absorber, and 0.2 to 0.5 parts of antioxidant.

[0006] Furthermore, the polyvinylidene fluoride is a copolymer of vinyl fluoride monomer and trifluoroethylene monomer, with a mass ratio of 3:1.

[0007] Furthermore, the inorganic nanofiller is nano magnesium sulfate, which is pretreated by ultrasonic cavitation and has a particle size of 100nm to 200nm.

[0008] Furthermore, the organic ultraviolet absorber is a mixture of benzophenone and benzotriazole in a mass ratio of 1:1.

[0009] Furthermore, the antioxidant is a mixture of hindered phenol and phosphite in a mass ratio of 2:1.

[0010] Furthermore, the POE is selected from one or more of ethylene-butene copolymer, ethylene-hexene copolymer and ethylene-octene copolymer.

[0011] Furthermore, the peroxide is selected from one or more of dicumyl peroxide, benzoyl peroxide, and 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane.

[0012] Furthermore, a method for preparing a low temperature resistant and tear resistant film comprises the following preparation steps:

[0013] (1) mixing 1-5 parts of an inorganic nanofiller, 80-100 parts of POE, 0.2-0.5 parts of an antioxidant, 0.1-0.5 parts of an inhibitor of crosslinking, and 1-2 parts of a lubricant, heating and melting, performing ultrasonic cavitation treatment during melting by an ultrasonic control device, and extruding by a twin-screw machine to obtain POE-nano functionalized particles;

[0014] (2) 1-5 parts of maleic anhydride, 0.2-0.5 parts of antioxidant, 0.1-0.5 parts of peroxide, 0.1-0.5 parts of crosslinking inhibitor, 1-2 parts of lubricant and the POE-nano functionalized particles prepared in step (1) are uniformly mixed by a high-speed mixer, and then ultrasonically treated and extruded to obtain a maleic anhydride grafted polyolefin elastomer;

[0015] (3) mixing 20 to 40 parts of polymethyl methacrylate, 1 to 5 parts of maleic anhydride grafted polyolefin elastomer, 1 to 3 parts of an organic ultraviolet absorber, and 0.2 to 0.5 parts of an antioxidant, and extruding and granulating the mixture through a twin-screw extruder to obtain a masterbatch;

[0016] (4) 50 to 80 parts of polyvinylidene fluoride are mixed with the master batch, and extruded and cast by a twin-screw extruder to prepare a low-temperature tear-resistant film with a thickness of 25 μm.

[0017] Furthermore, the ultrasonic power of step (1) is 600-1000W; and the ultrasonic frequency of step (2) is 200-600W.

[0018] Furthermore, in step (3), the extrusion temperature is 170°C and the mixing speed is 150 rpm; in step (4), the twin-screw extruder temperature is 240°C, the speed is 110 rpm, and the casting roll cooling temperature is 50°C.

[0019] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0020] The invention adopts the technical means of blending and modification, uses vinylidene fluoride homopolymer generated by polymerization of vinyl fluoride and trifluoroethylene as monomers as a matrix material, introduces maleic anhydride grafted polyolefin elastomer, and adopts nano-magnesium sulfate as a filler to mix, extrude and cast to prepare a film. The invention causes the maleic anhydride grafted polyolefin elastomer to undergo a grafting reaction with the surface of the nano-magnesium sulfate, improves the compatibility of the inorganic nano-filler with polyvinylidene fluoride, improves the dispersion degree of the nano-magnesium sulfate in the polyvinylidene fluoride, and the nano-magnesium sulfate is evenly dispersed in the polyvinylidene fluoride and can also play a certain toughening effect, thereby improving the impact resistance of the polyvinylidene fluoride.

[0021] The invention makes maleic anhydride grafted polyolefin elastomer and organic ultraviolet absorber undergo grafting reaction, thereby improving the compatibility of organic ultraviolet absorber and polyvinylidene fluoride, improving the disadvantage of easy migration and precipitation of organic ultraviolet absorber, and making the film maintain long-term ultraviolet resistance and low temperature resistance.

[0022] The invention does not pre-treat the nanoparticles with a solvent for a long time, but utilizes the cavitation effect of ultrasound to directly use maleic anhydride as a carrier to introduce free radicals, obtains maleic anhydride-nanoparticle functionalized masterbatch through a twin-screw extruder, and uses the masterbatch to carry out subsequent grafting experiments, thereby avoiding the disadvantages of easy agglomeration and difficult dispersion of the nanoparticles.

[0023] The present invention uses nano magnesium sulfate. When the ultrasonic waveform frequency is high, a large number of cavitation bubbles are formed. The bubbles wrap the nano magnesium sulfate and form a core-shell structure with maleic anhydride in a molten state. The soft shell (maleic anhydride) and the hard core (nanomagnesium sulfate) introduce free radicals. Since there are a large number of charges on the surface of the nanoparticles, the generation of the core-shell structure can be promoted. In the subsequent film toughening process, this structure can play a role of internal lubrication, thereby improving fluidity; on the other hand, due to the presence of the hard core, when impacted, it can better absorb energy, improve impact strength, and enhance tear resistance. DETAILED DESCRIPTION

[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0025] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the low temperature resistant and tear resistant plastic films prepared in the following examples are as follows:

[0026] Brittle temperature: Test method refers to GB / T5470

[0027] Impact strength: Test method refers to GB / T 1043.1

[0028] Tear strength: GB / T20218—2006

[0029] Example 1

[0030] (1) 3 parts of nano magnesium sulfate, 100 parts of POE, 0.5 parts of antioxidant, 0.3 parts of crosslinking inhibitor, and 2 parts of lubricant are mixed, heated and melted, ultrasonic cavitation treatment is performed during melting by an ultrasonic control device, and POE-nano functionalized particles are obtained by extruding through a twin-screw machine;

[0031] (2) 5 parts of maleic anhydride, 0.5 parts of antioxidant, 0.1 parts of peroxide, 0.5 parts of crosslinking inhibitor, and 2 parts of lubricant are mixed uniformly with the POE-nano functionalized particles prepared in step (1) by a high-speed mixer, and then subjected to ultrasonic treatment and extrusion to obtain a maleic anhydride grafted polyolefin elastomer;

[0032] (3) 40 parts of polymethyl methacrylate, 1 part of maleic anhydride grafted polyolefin elastomer, 1 part of organic ultraviolet absorber, and 0.2 parts of antioxidant were mixed, and extruded and granulated by a twin-screw extruder to obtain a masterbatch. The extrusion temperature was 170° C. and the mixing speed was 150 rpm.

[0033] (4) 70 parts of polyvinylidene fluoride were mixed with the master batch, and extruded and casted by a twin-screw extruder to obtain a low-temperature tear-resistant film with a thickness of 25 μm. The extruder temperature was 240° C., the rotation speed was 110 rpm, and the cooling temperature of the casting roller was 50° C.

[0034] Example 2

[0035] (1) 3 parts of nano magnesium sulfate, 100 parts of POE, 0.5 parts of antioxidant, 0.3 parts of crosslinking inhibitor, and 2 parts of lubricant are mixed, heated and melted, ultrasonic cavitation treatment is performed during melting by an ultrasonic control device, and POE-nano functionalized particles are obtained by extruding through a twin-screw machine;

[0036] (2) 5 parts of maleic anhydride, 0.5 parts of antioxidant, 0.1 parts of peroxide, 0.5 parts of crosslinking inhibitor, and 2 parts of lubricant are mixed uniformly with the POE-nano functionalized particles prepared in step (1) by a high-speed mixer, and then subjected to ultrasonic treatment and extrusion to obtain a maleic anhydride grafted polyolefin elastomer;

[0037] (3) 40 parts of polymethyl methacrylate, 5 parts of maleic anhydride grafted polyolefin elastomer, 1 part of organic ultraviolet absorber, and 0.2 parts of antioxidant were mixed, and extruded and granulated by a twin-screw extruder to obtain a masterbatch. The extrusion temperature was 170° C. and the mixing speed was 150 rpm.

[0038] (4) 70 parts of polyvinylidene fluoride were mixed with the master batch, and extruded and casted by a twin-screw extruder to obtain a low-temperature tear-resistant film with a thickness of 25 μm. The extruder temperature was 240° C., the rotation speed was 110 rpm, and the cooling temperature of the casting roller was 50° C.

[0039] Example 3

[0040] (1) 3 parts of nano magnesium sulfate, 100 parts of POE, 0.5 parts of antioxidant, 0.3 parts of crosslinking inhibitor, and 2 parts of lubricant are mixed, heated and melted, ultrasonic cavitation treatment is performed during melting by an ultrasonic control device, and POE-nano functionalized particles are obtained by extruding through a twin-screw machine;

[0041] (2) 5 parts of maleic anhydride, 0.5 parts of antioxidant, 0.1 parts of peroxide, 0.5 parts of crosslinking inhibitor, and 2 parts of lubricant are mixed uniformly with the POE-nano functionalized particles prepared in step (1) by a high-speed mixer, and then subjected to ultrasonic treatment and extrusion to obtain a maleic anhydride grafted polyolefin elastomer;

[0042] (3) 40 parts of polymethyl methacrylate, 5 parts of maleic anhydride grafted polyolefin elastomer, 3 parts of organic ultraviolet absorber, and 0.5 parts of antioxidant were mixed, and extruded and granulated by a twin-screw extruder to obtain a masterbatch. The extrusion temperature was 170° C. and the mixing speed was 150 rpm.

[0043] (4) 70 parts of polyvinylidene fluoride were mixed with the masterbatch, and extruded and casted by a twin-screw extruder to obtain a low-temperature tear-resistant film with a thickness of 25 μm. The extruder temperature was 240° C., the rotation speed was 110 rpm, and the casting roller cooling temperature was 50° C.

[0044] Comparative Example 1

[0045] The difference between Comparative Example 1 and Example 1 is that step (3) is different. Step (3) is changed to mixing 30 parts of polymethyl methacrylate, 5 parts of maleic anhydride grafted polyolefin elastomer, 3 parts of organic ultraviolet absorber, and 0.5 parts of antioxidant, and extruding and granulating through a twin-screw extruder to obtain a masterbatch. The extrusion temperature is 170°C and the mixing speed is 150rpm.

[0046] Comparative Example 2

[0047] The difference between Comparative Example 1 and Example 1 is that step (3) is different. Step (3) is changed to a mixture of 40 parts of polymethyl methacrylate, 1 part of inorganic nano-magnesium sulfate filler, 1 part of organic ultraviolet absorber, and 0.2 parts of antioxidant, and then extruded and granulated by a twin-screw extruder to obtain a masterbatch. The extrusion temperature is 170°C and the mixing speed is 150rpm.

[0048] Effect example

[0049] Table 1 below shows the performance analysis results of the low temperature resistant and tear resistant films of Examples 1 to 3 of the present invention and Comparative Examples 1 to 2.

[0050] Table 1

[0051] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Brittle temperature,℃ -54 -53 -49 -47 -45 <![CDATA[Impact strength, J / m 2 > 842 786 456 568 706 Tensile strength, MPa 269 254 260 240 216

[0052] From the data of the embodiments and comparative examples, it can be found that the present invention adopts the technical means of blending and modification, uses vinylidene fluoride homopolymer generated by polymerization of vinyl fluoride and trifluoroethylene as monomers as the matrix material, introduces maleic anhydride grafted polyolefin elastomer, and adopts nano-magnesium sulfate as filler to mix, extrude and cast to prepare the film. Maleic anhydride grafted polyolefin elastomer and nano-magnesium sulfate surface undergo grafting reaction, improves the compatibility of inorganic nano-filler and polyvinylidene fluoride, improves the dispersion degree of nano-magnesium sulfate in polyvinylidene fluoride, and nano-magnesium sulfate is uniformly dispersed in polyvinylidene fluoride, which can also play a certain toughening effect, thereby improving the impact resistance and tear resistance of polyvinylidene fluoride.

[0053] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A low temperature resistant and tear resistant film, characterized in that: The low-temperature resistant and tear-resistant film components include, by mass percentage, 50 to 80 parts of polyvinylidene fluoride, 20 to 40 parts of polymethyl methacrylate, 80 to 100 parts of polyethylene oxide (POE), 1 to 5 parts of maleic anhydride, 1 to 5 parts of inorganic nanofiller, 1 to 3 parts of organic ultraviolet absorber, 0.2 to 0.5 parts of antioxidant, 0.1 to 0.5 parts of peroxide, 0.1 to 0.5 parts of cross-linking inhibitor, and 1 to 2 parts of lubricant.

2. A low temperature resistant and tear resistant film according to claim 1, characterized in that: The polyvinylidene fluoride is a copolymer of vinyl fluoride monomer and trifluoroethylene monomer, with a mass ratio of 3:

1.

3. The low temperature resistant and tear resistant film according to claim 1, characterized in that: The inorganic nano filler is nano magnesium sulfate, which is pretreated by ultrasonic cavitation and has a particle size of 100nm to 200nm.

4. The low temperature resistant and tear resistant film according to claim 1, characterized in that: The organic ultraviolet absorber is a mixture of benzophenone and benzotriazole in a mass ratio of 1:

1.

5. The low temperature resistant and tear resistant film according to claim 1, characterized in that: The antioxidant is a mixture of hindered phenol and phosphite in a mass ratio of 2:

1.

6. The low temperature resistant and tear resistant film according to claim 1, characterized in that: The POE is selected from one or more of ethylene-butene copolymer, ethylene-hexene copolymer and ethylene-octene copolymer.

7. The low temperature resistant and tear resistant film according to claim 1, characterized in that: The peroxide is selected from one or more of dicumyl peroxide, benzoyl peroxide, and 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane.

8. A method for preparing a low temperature resistant and tear resistant film, characterized in that: The method comprises the following preparation steps: (1) mixing 1-5 parts of an inorganic nanofiller, 80-100 parts of POE, 0.2-0.5 parts of an antioxidant, 0.1-0.5 parts of an inhibitor of crosslinking agent, and 1-2 parts of a lubricant, heating and melting, performing ultrasonic cavitation treatment during melting by an ultrasonic control device, and extruding by a twin-screw machine to obtain POE-nano functionalized particles; (2) 1-5 parts of maleic anhydride, 0.2-0.5 parts of antioxidant, 0.1-0.5 parts of peroxide, 0.1-0.5 parts of crosslinking inhibitor, 1-2 parts of lubricant and the POE-nano functionalized particles prepared in step (1) are uniformly mixed by a high-speed mixer, and then ultrasonically treated and extruded to obtain a maleic anhydride grafted polyolefin elastomer; (3) mixing 20 to 40 parts of polymethyl methacrylate, 1 to 5 parts of maleic anhydride grafted polyolefin elastomer, 1 to 3 parts of an organic ultraviolet absorber, and 0.2 to 0.5 parts of an antioxidant, and extruding and granulating the mixture through a twin-screw extruder to obtain a masterbatch; (4) 50 to 80 parts of polyvinylidene fluoride are mixed with the master batch, and extruded and cast by a twin-screw extruder to obtain a low-temperature tear-resistant film with a thickness of 25 μm.

9. The method for preparing a low temperature resistant and tear resistant film according to claim 8, characterized in that: The ultrasonic power of step (1) is 600-1000W; the ultrasonic frequency of step (2) is 200-600W.

10. The method for preparing a low temperature resistant and tear resistant film according to claim 8, characterized in that: In step (3), the extrusion temperature is 170° C. and the mixing speed is 150 rpm; in step (4), the temperature of the twin-screw extruder is 240° C., the speed is 110 rpm, and the cooling temperature of the casting roll is 50° C.

Citation Information

Patent Citations

  • Nanoparticle-maleicanhydride composite grafted polyolefin elastomer and preparation method thereof

    CN104592450A

  • Low-temperature-resistant, ultraviolet-resistant and impact-resistant transparent fluorine-containing polymer film

    CN117801444A

  • Mono-layer pvdf film and preparation method thereof

    KR1020110119417A