Color master batch for refrigerator plate and preparation method of color master batch

By using materials such as HIPS, SBS elastomers and modified lignin in refrigerator sheets, combined with epoxy polysiloxoborane grafted modified lignin, the problems of poor mechanical properties and unstable double bond structure of refrigerator sheets are solved. It achieves good toughening and weather resistance, and improves the overall performance of the board.

CN119060486APending Publication Date: 2024-12-03HEFEI HEYUYA PLASTIC CHEM CO LTD

Patent Information

Application Number
CN202411185052.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The mechanical properties of refrigerator sheets are poor, especially ABS materials are susceptible to corrosion by hydrogenated fluorocarbon foaming agents, resulting in cracking and other adverse effects. The addition of recycled materials in HIPS materials reduces toughness, and the unstable double bond structure leads to aging and degradation of the material.

Method used

Using a color masterbatch for refrigerator sheets, including HIPS, SBS elastomer, modified lignin and titanium dioxide, the lignin is improved by epoxy polysiloxoborane grafting of lignin to improve the toughness and weather resistance of the material and enhance the material. dispersion and stability.

Benefits of technology

It effectively improves the toughening effect and weather resistance of refrigerator boards, improves impact and heat resistance, solves the material degradation problem caused by instability in the double bond structure, and ensures the mechanical properties and weather resistance of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005013271470000071
    Figure BDA0005013271470000071
  • Figure BDA0005013271470000081
    Figure BDA0005013271470000081
Patent Text Reader

Abstract

The invention discloses a color master batch for refrigerator plates and a preparation method thereof, and belongs to the technical field of color master batches, the color master batch comprises 20 parts of HIPS, 45-55 parts of SBS elastomer, 20-22 parts of titanium dioxide, 5-8 parts of modified lignin, 8-9 parts of a softening agent, and 0.5 part of a coloring agent; the modified lignin is epoxy polysiloxane borane grafted modified lignin; the preparation method comprises the following steps: putting the HIPS, the SBS elastomer, the titanium dioxide, the modified lignin and the coloring agent into a high-speed mixer, stirring and mixing, slowly adding the softening agent, stirring at 100 DEG C for 15 minutes, cooling, and extruding and granulating to obtain the color master batch for the refrigerator plate. The color master batch is endowed with good toughening effect and weather resistance by adding the SBS elastomer and the modified lignin, and can be effectively used for preparing an HIPS (High Impact Polystyrene) plate for a refrigerator so as to prepare the plate for the refrigerator with excellent performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of masterbatches, and in particular relates to a masterbatch for refrigerator plates and a preparation method thereof. Background Art

[0002] Blister products such as refrigerator liner and door panels are usually made of HIPS (high impact polystyrene) extruded sheets or acrylonitrile-butadiene-styrene terpolymer ABS (A represents acrylonitrile, B represents butadiene, and S represents styrene) extruded sheets through secondary processing and blister forming. Among them, the cost of ABS liner is relatively high, and ABS material is not resistant to corrosion by hydrofluorocarbon (HFC) foaming agents or mixed foaming systems containing HFC foaming agents, which can easily cause adverse effects such as cracking, and there is a high quality risk. HIPS (high impact polystyrene) extruded sheets are relatively low in cost and are usually made of HIPS, masterbatch and recycled materials. The addition of recycled materials will reduce the toughness of the sheet. In order to improve the toughness of the sheet, a toughening agent can be directly added to blend and prepare the sheet.

[0003] A special HIPS plate toughening masterbatch for refrigerators, a preparation method and application thereof are disclosed in the patent application with publication number CN106589745A. The special HIPS plate toughening masterbatch for refrigerators includes, by weight, 20-30 parts of main material, 25-35 parts of styrene-butadiene-styrene block copolymer toughening agent, 8-12 parts of white oil, 25-30 parts of titanium dioxide, 0.5-2 parts of pigment, and 3-5 parts of dispersant. The qualified rate of refrigerator plates prepared by the masterbatch is greatly improved, and the cost can be effectively reduced compared with the use of imported products. The SBS (styrene-butadiene-styrene block copolymer) in the formula is often used as a carrier resin to improve the toughness of HIPS, but the double bond structure in the material is an unstable structure, which is easily aged due to factors such as light, heat, and oxygen during the processing process and actual application, and is easily broken by double bonds when heated and strongly sheared, causing the material to degrade. The processed plates are easy to discolor and crack, which affects the mechanical properties and weather resistance of the finished products. Summary of the invention

[0004] The object of the present invention is to provide a masterbatch for refrigerator plates and a preparation method thereof, so as to solve the problem that the mechanical properties of refrigerator plates are poor.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A masterbatch for refrigerator plates comprises the following raw materials, measured by weight: 20 parts of HIPS, 45-55 parts of SBS elastomer, 20-22 parts of titanium dioxide, 5-8 parts of modified lignin, 8-9 parts of softener, and 0.5 parts of colorant; the modified lignin is epoxy polysiloxane grafted modified lignin.

[0007] In some possible implementations, the modified lignin is prepared by the following steps:

[0008] The hydroxymethylated modified lignin was added to a sodium hydroxide aqueous solution with a mass fraction of 1%, and then epoxy polysiloxane was added to react at a temperature of 30-35°C for 4 hours. After the reaction, the modified lignin was washed with water and dried to obtain the modified lignin. In the preparation process of the modified lignin, the epoxy group was introduced by the silane coupling agent KH-560 to participate in the grafting, and the phenyl group was introduced by phenylboronic acid to improve the compatibility of the modified lignin with the matrix, and the SiOBO chain segment with flexibility and high thermal stability was used to further improve the toughening effect of the masterbatch. The hydroxymethylated modified lignin was selected as the raw material to improve the efficiency of the grafting reaction between the hydroxymethylated modified lignin and epoxy polysiloxane, and the chain segment of epoxy polysiloxane was introduced into the structure of the lignin, which improved the dispersibility of the modified lignin in the HIPS matrix.

[0009] In some possible implementations, the mass ratio of the hydroxymethylated modified lignin to epoxy polysiloxane is 3:10.

[0010] In some possible implementations, the epoxy polysiloxane is prepared by the following steps:

[0011] Under nitrogen protection, phenylboric acid and dichloroethane were mixed, stirred and dissolved, KH-560 was added, the temperature was raised to 80°C for reaction for 8 hours, after the reaction was completed, the temperature was lowered to 20°C, and the mixture was allowed to stand for 8 hours. Excess phenylboric acid was removed by filtration, washed, and the solvent was removed by rotary evaporation. The mixture was vacuum dried at 60°C for 3 hours to obtain epoxy polysiloxane.

[0012] In some possible implementations, the molar ratio of phenylboric acid to KH-560 is 1.5:1.

[0013] In some possible implementations, the titanium dioxide is titanium dioxide with its surface coated with an organic substance: the organic substance is at least one of stearic acid, a titanate coupling agent, an aluminate coupling agent, and a silane coupling agent.

[0014] In some possible implementations, the hydroxymethylated modified lignin is prepared by the following steps:

[0015] Alkali lignin was dissolved with 1 mol / L sodium hydroxide solution, the pH of the solution was adjusted to 11, formaldehyde was added after heating in a water bath to reach the reaction temperature, the reaction was continued for 3 hours and then cooled, the pH of the solution was adjusted to 3 with 12% mass fraction hydrochloric acid, the precipitated lignin was centrifuged and washed with water to remove impurities, and finally dried in a 50°C forced air drying oven to obtain hydroxymethylated modified lignin.

[0016] In some possible implementations, the mass ratio of the alkali lignin to formaldehyde is 3-6:1;

[0017] The reaction temperature is 80-90°C.

[0018] In some possible implementations, the softener is white oil or naphthenic oil;

[0019] The colorant is an inorganic pigment, an organic pigment, a dye or a fluorescent brightener; the inorganic pigment is one or more of carbon black, ultramarine, cobalt blue, iron red, cadmium red, molybdenum chrome red, chrome yellow, aluminum powder and bronze powder; the organic pigment is one or more of phthalocyanine pigments and azo pigments.

[0020] A method for preparing masterbatch for refrigerator plate materials comprises the following steps:

[0021] Put HIPS, SBS elastomer, titanium dioxide, modified lignin and colorant into a high-speed mixer, stir and mix, slowly add softener, stir at 100°C for 15 minutes, cool, and granulate by extrusion to obtain masterbatch for refrigerator panels.

[0022] In some possible implementations, the temperature range of the feeding section of the extrusion granulation is 150°C-170°C, the temperature range of the melting section is 170°C-180°C, the temperature range of the plasticizing section is 180°C-195°C, and the temperature range of the die head zone is 200°C.

[0023] Beneficial effects of the present invention:

[0024] The invention provides a masterbatch for refrigerator plates. The masterbatch is endowed with good toughening effect and weather resistance by adding SBS elastomer and modified lignin, and can be effectively used in the preparation of HIPS plates for refrigerators to prepare refrigerator plates with excellent performance.

[0025] The main components of the masterbatch in the present invention include HIPS and SBS elastomers. As a thermoplastic elastomer, SBS elastomer has the properties of both rubber and plastic. It is easy to blend with plastic after heating and melting, and its elastomer properties can be restored after cooling. In addition, SBS elastomer has good compatibility with HIPS and has a good toughening effect. In the present invention, the impact resistance is further improved by increasing the proportion of SBS elastomer.

[0026] The structures of the SBS elastomer and HIPS in the present invention both contain butadiene components. Butadiene contains a double bond structure and has good compatibility, which can make the material have good toughness. In order to solve the problem that the double bond structure is unstable and the double bond is easily broken when heated and strongly sheared, resulting in material degradation, the modified lignin in the present invention is used as an anti-aging additive, which has the advantages of resistance to migration and extraction, etc. Compared with small molecule antioxidants and light stabilizers, the modified lignin in the present invention has higher stability.

[0027] In addition, the modified lignin in the present invention is modified by epoxy polysiloxane grafting and can withstand higher processing temperatures. Compared with the method of directly adding lignin, the self-made modified lignin in the present invention (epoxy polysiloxane grafted modified lignin) has better dispersibility in the masterbatch raw material. The reason is that HIPS and SBS elastomers are both non-polar materials, while lignin is a polar material, which is prone to agglomeration and uneven dispersion problems, directly affecting the toughening and weather resistance of the product. DETAILED DESCRIPTION

[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] The same products are compared in the embodiment and the comparative example, wherein HIPS is selected as HIPS-2710; SBS is selected as SBS brand 4402; the titanium dioxide is titanium dioxide with its surface coated by organic matter: the organic matter is stearic acid.

[0030] Preparation Example Preparation of modified lignin

[0031] Step S11, under nitrogen protection, 15 mmol phenylboric acid and 30 mL dichloroethane were mixed and stirred to dissolve in proportion, 10 mmol KH-560 (diluted with 30 mL dichloroethane) was added, the temperature was raised to 80 ° C. and the reaction was carried out for 8 hours. After the reaction was completed, the temperature was lowered to 20 ° C. and allowed to stand for 8 hours. The excess phenylboric acid was removed by suction filtration, washed, and the solvent was removed by rotary evaporation. The epoxy polysiloxane was dried in vacuo at 60 ° C. for 3 hours to obtain epoxy polysiloxane.

[0032] Step S12, dissolving the alkali lignin with 1 mol / L sodium hydroxide solution, adjusting the solution pH to 11, adding formaldehyde after heating in a water bath to the reaction temperature, reacting for 3 hours and then cooling, adjusting the solution pH to 3 with 12% mass fraction hydrochloric acid, centrifuging the precipitated lignin and washing with water to remove impurities, and finally drying in a 50°C forced air drying oven to obtain hydroxymethylated modified lignin. Wherein, the mass ratio of alkali lignin to formaldehyde is 3:1; and the reaction temperature is 80-90°C.

[0033] Step S13, adding the hydroxymethyl modified lignin to a sodium hydroxide aqueous solution with a mass fraction of 1%, and then adding epoxy polysiloxane to react at a temperature of 30-35°C for 4 hours. After the reaction is completed, washing and drying are performed to obtain modified lignin. The mass ratio of the hydroxymethyl modified lignin to the epoxy polysiloxane is 3:10, and the mass ratio of the hydroxymethyl modified lignin to the sodium hydroxide aqueous solution with a mass fraction of 1% is 1:10.

[0034] Preparation Example 2

[0035] The difference between this preparation example and preparation example 1 is:

[0036] In step S12, the mass ratio of alkali lignin to formaldehyde is 4:1.

[0037] Preparation Example 3

[0038] The difference between this preparation example and preparation example 1 is:

[0039] In step S12, the mass ratio of alkali lignin to formaldehyde is 5:1.

[0040] Preparation Example 4

[0041] The difference between this preparation example and preparation example 1 is:

[0042] In step S12, the mass ratio of alkali lignin to formaldehyde is 6:1.

[0043] Example 1

[0044] A method for preparing masterbatch for refrigerator plate materials comprises the following steps:

[0045] According to weight parts, 20 parts of HIPS, 45 parts of SBS elastomer, 20 parts of titanium dioxide, 5 parts of modified lignin (epoxy polysiloxane borane grafted modified lignin prepared in Test Example 1) and 0.5 parts of carbon black are put into a high mixer and stirred and mixed, 8 parts of white oil are slowly added, stirred at 100°C for 15 minutes, cooled, and extruded and granulated to obtain masterbatch for refrigerator sheet; the temperature range of the feeding section of the extrusion granulation is 150°C-170°C, the temperature range of the melting section is 170°C-180°C, the temperature range of the plasticizing section is 180°C-195°C, and the temperature range of the head zone is 200°C.

[0046] The difference between Example 2 to Example 5 and Example 1 is that the raw materials and their ratios are adjusted. The formulas of Example 1 to Example 5 are shown in Table 1 below:

[0047] Table 1

[0048] Example 1 Example 2 Example 3 Example 4 Example 5 HIPS 20 20 20 20 20 SBS Elastomer 45 50 51 54 55 Titanium dioxide 20 21 20 21 22 Modified lignin 5 6 6 7 8 Softener 8 8 8 9 9 Colorants 0.5 0.5 0.5 0.5 0.5

[0049] Example 6

[0050] The only difference between this example and Example 1 is that the modified lignin is replaced by the epoxy polysiloxane grafted modified lignin prepared in Test Example 2.

[0051] Example 7

[0052] The only difference between this example and Example 1 is that the modified lignin is replaced by the epoxy polysiloxane grafted modified lignin prepared in Test Example 3.

[0053] Example 8

[0054] The only difference between this example and Example 1 is that the modified lignin is replaced by the epoxy polysiloxane grafted modified lignin prepared in Test Example 4.

[0055] Comparative Example 1

[0056] The difference between this comparative example and Example 1 is that the modified lignin is replaced by a mixture of alkali lignin and epoxy polysiloxane in a mass ratio of 3:10 in Preparation Example 1.

[0057] Comparative Example 2

[0058] The only difference between this comparative example and Example 1 is that the modified lignin is replaced by alkali lignin.

[0059] Comparative Example 3

[0060] The difference between this comparative example and the example is that no modified lignin is added.

[0061] Performance testing

[0062] According to the ratio of HIPS: refrigerator plate masterbatch = 9:1, plate specimens were prepared and relevant properties were tested. Tensile strength and elongation at break: GB / T1040 plastic tensile properties test method; Flexural strength and flexural modulus: GB / T9341 plastic flexural properties test method; Notched impact strength: GB / T1843 plastic cantilever beam impact test method. The results are shown in Table 2 below:

[0063] Table 2

[0064]

[0065] The weather-resistant component (lignin) added in Comparative Example 1-Comparative Example 2 has a relatively poor dispersion effect with each component, which affects the improvement of the toughness of the sample. The samples prepared in Example 1-Example 8,

[0066] Aging performance test:

[0067] Test: The test samples were prepared according to the methods and proportions in Example 1 and Comparative Examples 1 to 3, and placed in an aging box. Light source: UV-B; wavelength: 313 nm; radiation intensity: 0.55 W / m 2 ; Cycle: 12h; Humidity: 65%; Cycle conditions: 60℃, light + no spray for 8h in the first stage, 50℃, no light + spray for 4h in the second stage. The change of notched impact strength after different cycles compared with the initial one is recorded, and the results are shown in Table 3 below

[0068] Table 3

[0069]

[0070] From the test results recorded in Table 2 and Table 3, it can be seen that the masterbatch for refrigerator plates added in the present invention has good toughening effect and weather resistance, and can be effectively used in the preparation of HIPS plates for refrigerators to prepare refrigerator plates with excellent performance.

[0071] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0072] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A masterbatch for refrigerator sheet material, characterized in that: The raw materials include the following in parts by weight: 20 parts of HIPS, 45-55 parts of SBS elastomer, 20-22 parts of titanium dioxide, 5-8 parts of modified lignin, 8-9 parts of softener, and 0.5 parts of colorant; the modified lignin is epoxy polysiloxane grafted modified lignin.

2. The masterbatch for refrigerator sheet material according to claim 1, characterized in that: The modified lignin is prepared by the following steps: The hydroxymethylated modified lignin was added into a sodium hydroxide aqueous solution with a mass fraction of 1%, and then epoxy polysiloxane was added to react at a temperature of 30-35° C. for 4 hours. After the reaction, the modified lignin was obtained by washing with water and drying.

3. A masterbatch for refrigerator sheet material according to claim 2, characterized in that: The mass ratio of the hydroxymethylated modified lignin to epoxy polysiloxane is 3:

10.

4. The masterbatch for refrigerator sheet material according to claim 1, characterized in that: The epoxy polysiloxane is prepared by the following steps: Under nitrogen protection, phenylboric acid and dichloroethane were mixed, stirred and dissolved, KH-560 was added, the temperature was raised to 80°C for reaction for 8 hours, after the reaction was completed, the temperature was lowered to 20°C, and the mixture was allowed to stand for 8 hours. Excess phenylboric acid was removed by filtration, washed, and the solvent was removed by rotary evaporation. The mixture was vacuum dried at 60°C for 3 hours to obtain epoxy polysiloxane.

5. The masterbatch for refrigerator sheet material according to claim 4, characterized in that: The molar ratio of the phenylboric acid to KH-560 is 1.5:

1.

6. The masterbatch for refrigerator sheet material according to claim 2, characterized in that: The hydroxymethylated modified lignin is prepared by the following steps: The alkali lignin was dissolved with 1 mol / L sodium hydroxide solution, the pH of the solution was adjusted to 11, formaldehyde was added after heating in a water bath to reach the reaction temperature, the reaction was continued for 3 hours and then cooled, the pH of the solution was adjusted to 3 with 12% mass fraction hydrochloric acid, the precipitated lignin was centrifuged and washed with water to remove impurities, and finally dried in a 50°C forced air drying oven to obtain hydroxymethylated modified lignin.

7. The masterbatch for refrigerator sheet material according to claim 6, characterized in that: The mass ratio of the alkali lignin to formaldehyde is 3-6:1; The reaction temperature is 80-90°C.

8. The masterbatch for refrigerator sheet material according to claim 1, characterized in that: The softener is white oil or naphthenic oil; The colorant is an inorganic pigment, an organic pigment, a dye or a fluorescent whitening agent; The titanium dioxide is titanium dioxide with its surface coated by organic matter: the organic matter is at least one of stearic acid, titanate coupling agent, aluminate coupling agent and silane coupling agent.

9. The method for preparing masterbatch for refrigerator plate according to claim 1, characterized in that: The steps include: Put HIPS, SBS elastomer, titanium dioxide, modified lignin and colorant into a high-speed mixer, stir and mix, slowly add softener, stir at 100°C for 15 minutes, cool, and granulate by extrusion to obtain masterbatch for refrigerator panels.

10. The method for preparing masterbatch for refrigerator plate according to claim 9, characterized in that: The temperature range of the feeding section of extrusion granulation is 150℃-170℃, the temperature range of the melting section is 170℃-180℃, the temperature range of the plasticizing section is 180℃-195℃, and the temperature range of the die head area is 200℃.

Citation Information

Patent Citations

  • Special HIPS panel toughening color masterbatch for refrigerator, preparation method and application thereof

    CN106589745A

Cited By

  • Weather-resistant color master batch and preparation method thereof

    CN119639127A