Styrene thermoplastic elastomer and preparation method thereof

Through the combination of low styrene content and high styrene content SBS blending and specific antioxidants, the problem of insufficient softness of styrene thermoplastic elastomers is solved, and the softness is improved on the basis of maintaining strength and wear resistance is achieved. and compatibility effects.

CN119060487APending Publication Date: 2024-12-03SHANDONG HAIRUIXIN NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411346416.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing styrene thermoplastic elastomers are not soft enough in some application scenarios, which affects their application in high-end shoe materials, baby products and certain medical devices. Adjusting the monomer ratio to improve softness will affect other materials. Properties such as tear strength and wear resistance.

Method used

Blend with low styrene content and high styrene content SBS and by using cycloane oil, calcium powder, zinc stearate, tetra[β-(3,5-di-tert-butyl-4-hydroxyphenyl) The combination of propionate]pentaerythritol ester antioxidant and tris(2,4-di-tert-butylphenyl)phosphite antioxidant improves the softness and compatibility of the material, ensuring strength and wear resistance.

Benefits of technology

On the basis of ensuring material strength and wear resistance, the softness of styrene-based thermoplastic elastomers is significantly improved, the compatibility problems caused by blending different SBSs is solved, and the product pass rate and performance balance is improved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a styrene thermoplastic elastomer and a preparation method thereof, and belongs to the field of chemical engineering. The styrene thermoplastic elastomer is prepared by blending two SBSs with different properties, and key parameters of the two SBSs are optimized, so that the softness of the elastomer is improved on the basis of not reducing the strength and wear resistance of the elastomer material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a styrene-based thermoplastic elastomer and a preparation method thereof, and belongs to the field of chemical industry. Background Art

[0002] Styrene thermoplastic elastomers (TPS), as an important branch of thermoplastic elastomers, have attracted much attention due to their unique physical and chemical properties and wide range of applications. This type of material is mainly made by copolymerization of styrene with other monomers such as butadiene, isoprene, etc., forming a block copolymer structure with alternating soft and hard phases. This structure gives styrene TPS excellent elasticity, wear resistance, low temperature resistance and good processing performance. Styrene TPS has a wide range of applications in multiple industrial fields. In the footwear industry, they are often used to make soles for sports shoes and ordinary shoes, providing excellent adhesion, low temperature flexibility and fatigue resistance. In the field of wires and cables, styrene TPS is used as insulation and sheath materials due to its good resilience and low temperature flexibility, which is competitive compared with cross-linked PE, vulcanized rubber, etc. In addition, in the automotive industry, styrene TPS is used to manufacture lightweight components such as seals, gaskets and hoses, which not only maintains high performance, but also reduces manufacturing costs and improves the fuel efficiency of automobiles. In the field of medical devices, polysiloxane-modified styrene block copolymers are widely used in the manufacture of products such as urinary implants, medical films and pacifiers due to their excellent biocompatibility and processing properties.

[0003] Although styrene thermoplastic elastomers have many advantages, their lack of softness has become a bottleneck that limits their application in certain specific application scenarios. Especially in areas that require high softness and good touch, such as high-end footwear, baby products and certain medical devices, the softness of the material is extremely high. In the prior art, one of the commonly used methods to improve the softness of styrene TPES is to adjust the monomer ratio of the copolymer and increase the content of the soft phase segment, such as increasing the proportion of butadiene or isoprene. However, although adjusting the monomer ratio can improve softness, it will affect other properties of the material such as tear strength and wear resistance. Therefore, the development of new soft styrene TPS materials and the exploration of more efficient and environmentally friendly methods to improve softness are still important directions of current research. Summary of the invention

[0004] In view of the above technical problems, the present invention achieves the goal of not reducing the strength and wear resistance of the material while ensuring the softness of TPS by blending two SBS with different properties, and solves the compatibility problem caused by two different SBS at the same time.

[0005] The present invention provides a styrene-based thermoplastic elastomer, which is composed of the following components: SBS with low styrene content, 10-20 parts; SBS with high styrene content, 2-6 parts; Naphthenic oil, 10-30 parts; Calcium powder, 10-20 parts; Zinc stearate, 0.2-0.8 parts; Pentaerythritol tetrakis[β-(3, 5-di-tert-butyl-4-hydroxyphenyl)propionate] antioxidant, 0.01-0.1 part; Tris(2,4-di-tert-butylphenyl)phosphite antioxidant, 0.01-0.1 parts; Among them, the styrene content of SBS with low styrene content is 20%-30%, the molecular weight is 140,000-160,000, and the melt flow index is 5-15 g / 10min (190℃ / 2.16kg); the styrene content of SBS with high styrene content is 35%-45%, the molecular weight is 110,000-130,000, and the melt flow index is 15-25 g / 10min (190℃ / 2.16kg).

[0006] Preferably, the cycloparaffinic oil is KN4010 oil.

[0007] The naphthenic oil is KN4010 oil.

[0008] The mesh size of the calcium powder is 500-2000 meshes.

[0009] The present invention also provides a method for preparing a styrene-based thermoplastic elastomer, which is characterized by comprising the following steps: (1) SBS with low styrene content is mixed with an appropriate amount of naphthenic oil to form material A; (2) SBS with a high styrene content is mixed with an appropriate amount of naphthenic oil to form material B; (3) Material A and material B are mixed, and calcium powder, zinc stearate, pentaerythritol tetrakis[β-(3, 5-di-tert-butyl-4-hydroxyphenyl) propionate antioxidant and tris(2,4-di-tert-butylphenyl) phosphite antioxidant are added, blended, stirred, and granulated to form a styrene-based thermoplastic elastomer.

[0010] Preferably, in step (1), the SBS with low styrene content is first mixed with the first portion of cyclohexane oil, stirred at 40-50°C for 30-40 minutes, and then the second portion of cyclohexane oil is added, and heating and stirring are continued. When the temperature of the mixed material reaches 40-50°C, the heating is turned off, and stirring is continued until the cyclohexane oil is completely absorbed.

[0011] Preferably, in step (2), the SBS with a high styrene content is mixed with the third portion of cyclohexane oil and stirred at 40-50°C. When the temperature of the mixed material reaches 40-50°C, the heating is turned off and stirring is continued until the cyclohexane oil is completely absorbed.

[0012] Preferably, the total of the first naphthenic oil, the second naphthenic oil and the third naphthenic oil is 10-30 parts; and the mass ratio of the first naphthenic oil, the second naphthenic oil and the third naphthenic oil is 8-12:8-12:1.

[0013] Preferably, the stirring is continued until the cyclohexane oil is completely absorbed for 2-6 hours.

[0014] Preferably, the stirring is continued until the cyclohexane oil is completely absorbed for 6-12 hours.

[0015] Preferably, the stirring time in step (3) is 2-5 minutes.

[0016] Compared with the prior art, the present invention has the following advantages: Firstly, the present invention adopts two SBS with different properties to blend and prepare styrene-based thermoplastic elastomer, and optimizes the key parameters of the two SBS, thereby improving the softness of the elastomer without reducing the strength and wear resistance of the elastomer material.

[0017] Secondly, since the performance of the two SBS is quite different, the present invention first mixes and absorbs the two SBS with naphthenic oils of different proportions and then blends them, thereby improving the qualified rate of the product and avoiding imbalance in product performance.

[0018] Finally, in order to solve the compatibility problem when two SBS with different properties are blended, the present invention adopts a combination of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] antioxidant and tris(2,4-di-tert-butylphenyl)phosphite antioxidant. On the basis of ensuring the antioxidant performance, the tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] antioxidant can stabilize the molecules at the phase interface, and the tris(2,4-di-tert-butylphenyl)phosphite antioxidant can react with the unsaturated bonds in the material to improve the compatibility of the material. The synergistic effect of the two ensures the antioxidant performance and compatibility. DETAILED DESCRIPTION

[0019] Example 1: The TPS elastomer of this example includes the following components: SBS with low styrene content, 16kg; SBS with high styrene content, 4kg; KN4010 white oil, 25.2kg; 1250 mesh calcium powder (GY-316), 16kg; Zinc stearate (BS-2818), 0.4kg; Pentaerythritol tetrakis[β-(3, 5-di-tert-butyl-4-hydroxyphenyl)propionate] antioxidant, 0.03 kg; Tris(2,4-di-tert-butylphenyl)phosphite antioxidant, 0.03kg; Among them, the styrene content of SBS with low styrene content is 25%, the molecular weight is 150,000, and the melt flow index is 10 g / 10min; the styrene content of SBS with high styrene content is 40%, the molecular weight is 120,000, and the melt flow index is 20 g / 10min.

[0020] The TPS elastomer of this embodiment is prepared by the following steps: (1) Put 16kg of SBS with low styrene content into the mixing tank, add 12kg of KN4010 oil evenly, and start stirring. Set the temperature to 45℃. After stirring for 30 minutes, add another 12kg of KN4010 oil evenly. When the temperature of the mixed material reaches 45℃, turn off the heating and continue stirring until the cyclohexane oil is completely absorbed.

[0021] (2) Mix 4kg of SBS with high styrene content with 1.2kg of KN4010 oil and stir at 45°C. When the temperature of the mixed material reaches 45°C, turn off the heating and continue stirring until the cyclohexane oil is completely absorbed.

[0022] (3) The material formed in step (1) and the material formed in step (2) are mixed, and 16 kg of calcium powder, 0.4 kg of zinc stearate, 0.03 kg of pentaerythritol tetrakis[β-(3, 5-di-tert-butyl-4-hydroxyphenyl) propionate antioxidant, and 0.03 kg of tris(2,4-di-tert-butylphenyl) phosphite antioxidant are added, blended, stirred, and granulated to form a styrene-based thermoplastic elastomer.

[0023] Comparative Example 1 The TPS elastomer of this comparative example comprises the following components: SBS with low styrene content, 20kg; KN4010 white oil, 25.2kg; 1250 mesh calcium powder (GY-316), 16kg; Zinc stearate (BS-2818), 0.4kg; Pentaerythritol tetrakis[β-(3, 5-di-tert-butyl-4-hydroxyphenyl)propionate] antioxidant, 0.03 kg; Tris(2,4-di-tert-butylphenyl)phosphite antioxidant, 0.03kg.

[0024] The TPS elastomer of this embodiment is prepared by the following steps: (1) Put 16kg of SBS with low styrene content into the mixing tank, add 12kg of KN4010 oil evenly, and start stirring. Set the temperature to 45℃. After stirring for 30 minutes, add another 12kg of KN4010 oil evenly. When the temperature of the mixed material reaches 45℃, turn off the heating and continue stirring until the cyclohexane oil is completely absorbed.

[0025] (2) Mix 4 kg of SBS with low styrene content with 1.2 kg of KN4010 oil and stir at 45°C. When the temperature of the mixed material reaches 45°C, turn off the heating and continue stirring until the cyclohexane oil is completely absorbed.

[0026] (3) The material formed in step (1) and the material formed in step (2) are mixed, and 16 kg of calcium powder, 0.4 kg of zinc stearate, 0.03 kg of pentaerythritol tetrakis[β-(3, 5-di-tert-butyl-4-hydroxyphenyl) propionate antioxidant, and 0.03 kg of tris(2,4-di-tert-butylphenyl) phosphite antioxidant are added, blended, stirred, and granulated to form a styrene-based thermoplastic elastomer.

[0027] Comparative Example 2: The TPS elastomer of this comparative example includes the following components: SBS with high styrene content, 20kg; KN4010 white oil, 25.2kg; 1250 mesh calcium powder (GY-316), 16kg; Zinc stearate (BS-2818), 0.4kg; Pentaerythritol tetrakis[β-(3, 5-di-tert-butyl-4-hydroxyphenyl)propionate] antioxidant, 0.03 kg; Tris(2,4-di-tert-butylphenyl)phosphite antioxidant, 0.03kg; The TPS elastomer of this embodiment is prepared by the following steps: (1) Put 16kg of SBS with high styrene content into the mixing tank, add 12kg of KN4010 oil evenly, and start stirring. Set the temperature to 45℃. After stirring for 30 minutes, add another 12kg of KN4010 oil evenly. When the temperature of the mixed material reaches 45℃, turn off the heating and continue stirring until the cyclohexane oil is completely absorbed.

[0028] (2) Mix 4 kg of SBS with high styrene content with 1.2 kg of KN4010 oil and stir at 45°C. When the temperature of the mixed material reaches 45°C, turn off the heating and continue stirring until the cyclohexane oil is completely absorbed.

[0029] (3) The material formed in step (1) and the material formed in step (2) are mixed, and 16 kg of calcium powder, 0.4 kg of zinc stearate, 0.03 kg of pentaerythritol tetrakis[β-(3, 5-di-tert-butyl-4-hydroxyphenyl) propionate antioxidant, and 0.03 kg of tris(2,4-di-tert-butylphenyl) phosphite antioxidant are added, blended, stirred, and granulated to form a styrene-based thermoplastic elastomer.

[0030] Comparative Example 3: The TPS elastomer of this embodiment includes the following components: SBS with low styrene content, 16kg; SBS with high styrene content, 4kg; KN4010 white oil, 25.2kg; 1250 mesh calcium powder (GY-316), 16kg; Zinc stearate (BS-2818), 0.4kg; Pentaerythritol tetrakis[β-(3, 5-di-tert-butyl-4-hydroxyphenyl)propionate] antioxidant, 0.03 kg; Tris(2,4-di-tert-butylphenyl)phosphite antioxidant, 0.03kg; The TPS elastomer of this comparative example was prepared by the following steps: (1) Put 16kg of SBS with low styrene content into the mixing tank, add 10.08kg of KN4010 oil evenly, and start stirring. Set the temperature to 45℃. After stirring for 30 minutes, add another 10.08kg of KN4010 oil evenly. When the temperature of the mixed material reaches 45℃, turn off the heating and continue stirring until the cyclohexane oil is completely absorbed.

[0031] (2) Mix 4kg of SBS with high styrene content with 5.04kg of KN4010 oil and stir at 45°C. When the temperature of the mixed material reaches 45°C, turn off the heating and continue stirring until the cyclohexane oil is completely absorbed.

[0032] (3) The material formed in step (1) and the material formed in step (2) are mixed, and 16 kg of calcium powder, 0.4 kg of zinc stearate, 0.03 kg of pentaerythritol tetrakis[β-(3, 5-di-tert-butyl-4-hydroxyphenyl) propionate antioxidant, and 0.03 kg of tris(2,4-di-tert-butylphenyl) phosphite antioxidant are added, blended, stirred, and granulated to form a styrene-based thermoplastic elastomer.

[0033] Comparative Example 4: The TPS elastomer of this comparative example includes the following components: SBS with low styrene content, 16kg; SBS with high styrene content, 4kg; KN4010 white oil, 25.2kg; 1250 mesh calcium powder (GY-316), 16kg; Zinc stearate (BS-2818), 0.4kg; Pentaerythritol tetrakis[β-(3, 5-di-tert-butyl-4-hydroxyphenyl)propionate] antioxidant, 0.03 kg; Tris(2,4-di-tert-butylphenyl)phosphite antioxidant, 0.03kg.

[0034] The TPS elastomer of this comparative example was prepared by the following steps: (1) Put 16kg of SBS with low styrene content into the mixing tank, evenly add 24kg of KN4010 oil, and start stirring. Set the temperature to 45℃. When the temperature of the mixed material reaches 45℃, turn off the heating and continue stirring until the cyclohexane oil is completely absorbed.

[0035] (2) Mix 4kg of SBS with high styrene content with 1.2kg of KN4010 oil and stir at 45°C. When the temperature of the mixed material reaches 45°C, turn off the heating and continue stirring until the cyclohexane oil is completely absorbed.

[0036] (3) The material formed in step (1) and the material formed in step (2) are mixed, and 16 kg of calcium powder, 0.4 kg of zinc stearate, 0.03 kg of pentaerythritol tetrakis[β-(3, 5-di-tert-butyl-4-hydroxyphenyl) propionate antioxidant, and 0.03 kg of tris(2,4-di-tert-butylphenyl) phosphite antioxidant are added, blended, stirred, and granulated to form a styrene-based thermoplastic elastomer.

[0037] Comparative Example 5: The TPS elastomer of this comparative example includes the following components: SBS with low styrene content, 16kg; SBS with high styrene content, 4kg; KN4010 white oil, 25.2kg; 1250 mesh calcium powder (GY-316), 16kg; Zinc stearate (BS-2818), 0.4kg; Pentaerythritol tetrakis[β-(3, 5-di-tert-butyl-4-hydroxyphenyl)propionate] antioxidant, 0.06kg.

[0038] The TPS elastomer of this comparative example was prepared by the following steps: (1) Put 16kg of SBS with low styrene content into the mixing tank, add 12kg of KN4010 oil evenly, and start stirring. Set the temperature to 45℃. After stirring for 30 minutes, add another 12kg of KN4010 oil evenly. When the temperature of the mixed material reaches 45℃, turn off the heating and continue stirring until the cyclohexane oil is completely absorbed.

[0039] (2) Mix 4kg of SBS with high styrene content with 1.2kg of KN4010 oil and stir at 45°C. When the temperature of the mixed material reaches 45°C, turn off the heating and continue stirring until the cyclohexane oil is completely absorbed.

[0040] (3) The material formed in step (1) and the material formed in step (2) were mixed, and 16 kg of calcium powder, 0.4 kg of zinc stearate, and 0.06 kg of pentaerythritol tetrakis[β-(3, 5-di-tert-butyl-4-hydroxyphenyl)propionate antioxidant were added, blended, stirred, and granulated to form a styrene-based thermoplastic elastomer.

[0041] Comparative Example 6: The TPS elastomer of this comparative example includes the following components: SBS with low styrene content, 16kg; SBS with high styrene content, 4kg; KN4010 white oil, 25.2kg; 1250 mesh calcium powder (GY-316), 16kg; Zinc stearate (BS-2818), 0.4kg; Tris(2,4-di-tert-butylphenyl)phosphite antioxidant, 0.06kg; Among them, the styrene content of SBS with low styrene content is 25%, the molecular weight is 150,000, and the melt flow index is 10 g / 10min; the styrene content of SBS with high styrene content is 40%, the molecular weight is 120,000, and the melt flow index is 20 g / 10min.

[0042] The TPS elastomer of this comparative example was prepared by the following steps: (1) Put 16kg of SBS with low styrene content into the mixing tank, add 12kg of KN4010 oil evenly, and start stirring. Set the temperature to 45℃. After stirring for 30 minutes, add another 12kg of KN4010 oil evenly. When the temperature of the mixed material reaches 45℃, turn off the heating and continue stirring until the cyclohexane oil is completely absorbed.

[0043] (2) Mix 4kg of SBS with high styrene content with 1.2kg of KN4010 oil and stir at 45°C. When the temperature of the mixed material reaches 45°C, turn off the heating and continue stirring until the cyclohexane oil is completely absorbed.

[0044] (3) The material formed in step (1) and the material formed in step (2) were mixed, and 16 kg of calcium powder, 0.4 kg of zinc stearate, and 0.06 kg of tris(2,4-di-tert-butylphenyl)phosphite antioxidant were added, blended, stirred, and granulated to form a styrene-based thermoplastic elastomer.

[0045] The samples of Example 1 and Comparative Examples 1-6 were characterized, and the standards included: (1) Use a Shore A hardness tester to test the hardness of the sample (Shore A); (2) Use the drainage method to test the specific gravity of the sample; (3) Use a melt index meter to test the melt index at 150℃ / 2.16KG; (4) Use a universal material testing machine to test the tensile strength and elongation at break of the sample; (5) Use a tear strength testing machine to perform a tear test on the sample to test the tear strength; (6) Use a wear testing machine to test the wear resistance index of the sample.

[0046] Specific characterization data are shown in Table 1: Table 1 Characterization results of different samples sample Hardness Shore A proportion Melt index (g / 10min) Tensile strength (MPa) Tear strength (KN / m) Elongation at break (%) Wear resistance index (mm³ / N·m) Real 1 15.3A 1.052 20.5 2.45 17.8 1245 19.7 1 17.6A 1.074 15.9 1.92 13.5 1090 14.3 2 12.8A 1.027 30.2 1.78 9.6 1302 11.4 3 16.1A 1.063 17.7 2.15 14.9 1048 12.8 4 14.9A 1.057 26.1 1.98 12.7 1175 13.9 5 15.6A 1.049 18.8 2.29 14.8 995 11.6 6 16.7A 1.058 21.9 2.06 11.3 1147 12.5 Although the specific embodiments of the present invention are described and illustrated in detail above, it should be pointed out that various equivalent changes and modifications can be made to the above embodiments based on the concept of the present invention. As long as the functional effects produced do not exceed the spirit covered by the specification, they should all be within the protection scope of the present invention.

Claims

1. A styrene-based thermoplastic elastomer, characterized in that It consists of the following components: SBS with low styrene content, 10-20 parts; SBS with high styrene content, 2-6 parts; Naphthenic oil, 10-30 parts; Calcium powder, 10-20 parts; Zinc stearate, 0.2-0.8 parts; Pentaerythritol tetrakis[β-(3, 5-di-tert-butyl-4-hydroxyphenyl)propionate] antioxidant, 0.01-0.1 part; Tris(2,4-di-tert-butylphenyl)phosphite antioxidant, 0.01-0.1 parts; Among them, the styrene content of SBS with low styrene content is 20%-30%, the molecular weight is 140,000-160,000, and the melt flow index is 5-15 g / 10min; the styrene content of SBS with high styrene content is 35%-45%, the molecular weight is 110,000-130,000, and the melt flow index is 15-25 g / 10min.

2. The elastic body according to claim 1, characterized in that The naphthenic oil is KN4010 oil.

3. The elastic body according to claim 1, characterized in that The mesh size of the calcium powder is 500-2000 meshes.

4. A method for preparing a styrene-based thermoplastic elastomer according to claim 1, characterized in that The steps include: (1) SBS with low styrene content is mixed with an appropriate amount of naphthenic oil to form material A; (2) SBS with a high styrene content is mixed with an appropriate amount of naphthenic oil to form material B; (3) Material A and material B are mixed, and calcium powder, zinc stearate, pentaerythritol tetrakis[β-(3, 5-di-tert-butyl-4-hydroxyphenyl) propionate antioxidant and tris(2,4-di-tert-butylphenyl) phosphite antioxidant are added, blended, stirred, and granulated to form a styrene-based thermoplastic elastomer.

5. The preparation method according to claim 4, characterized in that: In step (1), the SBS with low styrene content is first mixed with the first portion of cyclohexane oil, stirred at 40-50°C for 30-40 minutes, and then the second portion of cyclohexane oil is added, and heating and stirring are continued. When the temperature of the mixed material reaches 40-50°C, the heating is turned off and stirring is continued until the cyclohexane oil is completely absorbed.

6. The preparation method according to claim 5, characterized in that: In step (2), the SBS with a high styrene content is mixed with the third portion of cyclohexane oil and stirred at 40-50°C. When the temperature of the mixed material reaches 40-50°C, the heating is turned off and stirring is continued until the cyclohexane oil is completely absorbed.

7. The preparation method according to claim 6, characterized in that The total amount of the first naphthenic oil, the second naphthenic oil and the third naphthenic oil is 10-30 parts; and the mass ratio of the first naphthenic oil, the second naphthenic oil and the third naphthenic oil is 8-12:8-12:

1.

8. The preparation method according to claim 5, characterized in that The stirring is continued until the cyclohexane oil is completely absorbed for 2-6 hours.

9. The preparation method according to claim 6, characterized in that The stirring is continued until the naphthenic oil is completely absorbed for 6-12 hours.

10. The preparation method according to claim 4, characterized in that The stirring time in step (3) is 2-5 minutes.