Resin composition and product thereof
By using a polyphenylene ether resin containing unsaturated carbon-carbon double bonds and a compound of formula (1) with a pH value of 5 to 10 in the resin composition, a resin composition for a printed circuit board was solved The problem of insufficient performance of copper clad plates in the prior art has achieved higher density and stability and is suitable for high-frequency environments.
Patent Information
- Application Number
- CN202310626518.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-30
- Publication Date
- 2024-12-03
Smart Images

Figure CN119060524A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a resin composition and products made from the same, and in particular to a resin composition that can be used to prepare products such as prepregs, resin films, laminates or printed circuit boards. Background Art
[0002] As a basic electronic component, printed circuit boards (PCBs) are used in many fields including communications, industrial control, consumer electronics, automotive electronics, aerospace, etc. Their technical level has a direct impact on the technical stability and reliability of electronic equipment. With the development of technologies such as 5G and the Internet of Things, the transmission rate and frequency of signals have been greatly improved. As the substrate material of PCB, copper clad laminate (CCL, or copper foil substrate) mainly plays the role of interconnection, insulation and support for PCB, and has a great influence on the transmission speed, energy loss, characteristic impedance and other aspects of the signal in the circuit. The performance, quality, processability in manufacturing, long-term reliability, stability and other characteristics of PCB depend to a large extent on the quality of copper clad laminate.
[0003] The problems of process capability, signal integrity, heat dissipation and stress currently faced by advanced PCB packaging technology have put forward higher requirements for the performance of copper clad laminates: higher density (such as high-density multilayer boards), better and more stable electrical properties (such as lower dielectric loss aging rate, lower dielectric constant temperature coefficient TcDk and dielectric loss temperature coefficient TcDf), etc. However, existing copper clad laminates and their resin compositions still mainly focus on the general conventional properties of copper clad laminates.
[0004] Therefore, the art urgently needs to develop resin compositions and their copper-clad laminates and other products having excellent interconnect structure reliability, lower dielectric loss aging rate, lower dielectric constant temperature coefficient TcDk and dielectric loss temperature coefficient TcDf, while taking into account high-layer bonding strength, excellent filling properties, and resin and glass fiber interface adhesion. Summary of the invention
[0005] In view of the above-mentioned technical problems existing in the prior art, especially the problem that existing materials cannot meet one or more of the above-mentioned performance requirements, the main purpose of the present invention is to provide a resin composition that can overcome at least one of the above-mentioned technical problems, and a product made of the resin composition.
[0006] The first aspect of the present invention provides a resin composition comprising the following components or prepolymers thereof:
[0007] (A) 100 parts by weight of a polyphenylene ether resin containing unsaturated carbon-carbon double bonds;
[0008] (B) 10 to 50 parts by weight of a compound of formula (1), wherein the pH value of the compound of formula (1) is 5 to 10;
[0009]
[0010] In formula (1), n is an integer of 3 to 6, and X and Y are each independently o-vinylphenoxy or p-vinylphenoxy, and X and Y are not both o-vinylphenoxy and p-vinylphenoxy;
[0011] The prepolymer is obtained by prepolymerization of a mixture, and the mixture includes the component (A) and the component (B).
[0012] For example, in one embodiment, the prepolymer is formed by prepolymerization of the component (A) and the component (B), and the conversion rate of the prepolymerization is 10% to 99%.
[0013] For example, in one embodiment, the conversion rate of the prepolymerization reaction is 10% to 99%, preferably 30% to 95%, more preferably 50% to 90%, and further preferably 75% to 90%.
[0014] For example, in one embodiment, the polyphenylene ether resin containing unsaturated carbon-carbon double bonds includes any one of vinylbenzyl polyphenylene ether resin, (meth)acryl polyphenylene ether resin, vinyl polyphenylene ether resin, or a combination thereof. Preferably, the vinylbenzyl polyphenylene ether resin includes any one of vinylbenzyl biphenyl polyphenylene ether resin and vinylbenzyl bisphenol A polyphenylene ether resin, or a combination thereof.
[0015] For example, in one embodiment, the resin composition further comprises polyolefin, and the amount of the polyolefin is 5 to 25 parts by weight relative to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds. Preferably, the polyolefin includes any one of a diene polymer, a monoene polymer, a hydrogenated diene polymer, or a combination thereof.
[0016] For example, in one embodiment, the resin composition further comprises any one of bis(vinylphenyl)ethane, divinylbenzene, divinylnaphthalene, divinylbiphenyl, tert-butylstyrene, triallyl isocyanurate, triallyl cyanurate, vinylbenzocyclobutene, di(vinylbenzyl)ether, trivinylcyclohexane, diallyl isophthalate, diallyl bisphenol A, acrylate, butadiene, decadiene, octadiene, vinylcarbazole, and styrene, or a combination thereof.
[0017] For example, in one embodiment, the resin composition further comprises any one of epoxy resin, polyester resin, phenol resin, amine curing agent, polyamide, polyimide, styrene maleic anhydride, cyanate ester or a combination thereof.
[0018] For example, in one embodiment, the resin composition further comprises any one of an inorganic filler, a flame retardant, a hardening accelerator, an inhibitor, a solvent, a silane coupling agent, a colorant, and a toughening agent, or a combination thereof.
[0019] For example, in one embodiment, the resin composition further comprises a phosphate flame retardant, and the mass ratio of the compound of formula (1) to the phosphate flame retardant is between 1.5:1.0 and 25.0:1.0.
[0020] The present invention also provides a product made from the resin composition, wherein the product includes: a prepreg, a resin film, a laminate or a printed circuit board.
[0021] For example, in one embodiment, the article has one or more of the following characteristics:
[0022] The resistance change rate after 1000 cycles measured by the interconnect stress test according to IPC-TM-650 2.6.26 is less than 10%;
[0023] The interlayer bond strength measured according to IPC-TM-650 2.4.8 is greater than or equal to 3.5 lb / in;
[0024] The dielectric constant temperature coefficient measured according to IPC-TM-650 2.5.5.13 is less than or equal to 73ppm / ℃;
[0025] The dielectric loss temperature coefficient measured according to IPC-TM-650 2.5.5.13 is less than or equal to 6300ppm / ℃;
[0026] After the product is left to stand for 500 hours in an environment with a temperature of 85° C. and a relative humidity of 85%, the dielectric loss aging rate calculated by measuring the dielectric loss at a frequency of 10 GHz according to the method of JIS C2565 is less than or equal to 57%.
[0027] The resin composition and its products obtained by the present invention are improved in one or more aspects such as filling property, interconnection structure reliability, interface tightness between resin matrix and glass fiber, dielectric loss aging rate, interlayer bonding force, dielectric constant temperature coefficient TcDk, dielectric loss temperature coefficient TcDf, etc., which has achieved significant progress compared with the prior art. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is an example diagram showing a shadow on the copper-free surface of the inner circuit substrate that does not contain copper in the glue filling test according to the present invention;
[0029] Figure 2 It is an example diagram showing a shadow-free surface of an inner circuit substrate containing no copper in a test of the glue filling property according to the present invention;
[0030] Figure 3 It is an example diagram showing a gap between the resin composition and the warp or weft glass fibers in the interface adhesion test according to the present invention;
[0031] Figure 4 The figure shows an example of no gap between the resin composition and the warp or weft glass fibers in the interface adhesion test according to the present invention. DETAILED DESCRIPTION
[0032] In order to make those skilled in the art understand the characteristics and effects of the present application, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical terms used herein refer to the common meanings understood by those skilled in the art for the present application. In case of conflict, the definitions in this specification shall prevail.
[0033] The theories or mechanisms described and disclosed herein, whether or not they are scientifically confirmed, should not limit the scope of the present application in any way, that is, the content of the present application can be implemented without being limited by any specific theory or mechanism.
[0034] The use of "one", "an", "a kind" or similar expressions to describe the components and technical features described in this application is only for the convenience of expression and to provide a general meaning to the scope of this application. Therefore, this description should be understood to include one or at least one, and the singular also includes the plural, unless otherwise explicitly stated.
[0035] Herein, the terms "comprise", "include", "have", "contain" or any other similar terms are open conjunctions, which are intended to cover non-exclusive inclusions. For example, a composition or its product comprising multiple elements includes any one or any one of the listed elements, and is not limited to all the elements listed herein, but may also include other elements that are not explicitly listed but are generally inherent to the composition or its product. In addition, unless otherwise expressly stated, the term "or" refers to an inclusive "or" rather than an exclusive "or". For example, any of the following situations satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist), A is false (or does not exist) and B is true (or exists), and A and B are both true (or exist). In addition, in this article, the terms "comprising", "including", "having", and "containing" should be interpreted as specifically disclosed and simultaneously covering closed conjunctions such as "consisting of", "consisting of", "the remainder of", and conjunctions such as "consisting essentially of", "mainly consisting of", "mainly consisting of", "essentially containing", "essentially consisting of", "essentially consisting of", and "essentially containing".
[0036] As used herein, “or a combination thereof” means “or any combination thereof”, covering any combination of more than two of the listed elements; “any one”, “any one”, “any one” means “any one”, “any one”, “any one”. For example, “a composition or its product includes A, B, C or a combination thereof”, when interpreted, covers the following situations: A is true (or exists) and B and C are false (or do not exist), B is true (or exists) and A and C are false (or do not exist), C is true (or exists) and A and B are false (or do not exist), A and B are true (or exist) and C is false (or do not exist), A and C are true (or exist) and B is false (or do not exist), B and C are true (or exist) and A is false (or do not exist), A and C are true (or exist) and B is false (or do not exist), B and C are true (or exist) and A is false (or do not exist), A, B and C are all true (or exist), and other elements not explicitly listed but that are typically inherent to the composition or its product.
[0037] In this article, the terms "and", "and", "and", "as well as" or other similar terms are used to connect parallel sentence components, and there is no distinction between the previous and the next components. The grammatical meaning of the parallel sentence components does not change after the positions of the parallel sentence components are exchanged.
[0038] In this article, all features or conditions such as numerical values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are only concise and convenient. Accordingly, the description of numerical ranges or percentage ranges should be deemed to have covered and specifically disclosed all possible sub-ranges and individual values within the range (including integers and fractions), especially integer values. For example, the range description of "1.0 to 8.0", "between 1.0 and 8.0" or "between 1.0 to 8.0" should be deemed to have specifically disclosed all sub-ranges such as 1.0 to 8.0, 1.0 to 7.0, 2.0 to 8.0, 2.0 to 6.0, 3.0 to 6.0, 4.0 to 8.0, 3.0 to 8.0, and should be deemed to cover endpoint values, especially sub-ranges defined by integer values, and should be deemed to have specifically disclosed individual values such as 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, etc. Unless otherwise indicated, the foregoing method of interpretation applies to all contents of the entire application, regardless of whether the scope is broad or not.
[0039] If the quantity, concentration or other numerical value or parameter is expressed as a range, a preferred range (or a preferred range) or a series of upper and lower limits, it should be understood that all ranges consisting of any pair of the upper limit or preferred value (or a preferred value) of the range and the lower limit or preferred value (or a preferred value) of the range have been specifically disclosed herein, regardless of whether these ranges are disclosed separately. In addition, if a numerical range is mentioned herein, unless otherwise specified, the range includes its endpoints and all integers and fractions within the range.
[0040] Herein, numerical values should be understood to have the accuracy of the significant digits of the numerical value, provided that the purpose of the invention can be achieved. For example, the number 40.0 should be understood to cover the range of 39.50 to 40.49.
[0041] In this article, for the use of Markush groups or optional terms to describe the features or examples of the present application, those skilled in the art should understand that all subgroups or any individual elements in the Markush group or option list can also be used to describe the present application. For example, if x is described as "selected from the group consisting of X1, X2 and X3", it also means that the claim that X is X1 and the claim that X is X1 and / or X2 and / or X3 have been fully described. Furthermore, for the use of Markush groups or optional terms to describe the features or examples of the present application, those skilled in the art should understand that any combination of subgroups or individual members of all elements in the Markush group or option list can also be used to describe the present application. Accordingly, for example, if X is described as "selected from the group consisting of X1, X2 and X3", and Y is described as "selected from the group consisting of Y1, Y2 and Y3", it means that the claim that X is X1 and / or X2 and / or X3 and Y is Y1 and / or Y2 and / or Y3 has been fully described.
[0042] Unless otherwise specified, in this application, a compound refers to a chemical substance formed by two or more elements connected by chemical bonds, including small molecule compounds and polymer compounds, but not limited thereto. The interpretation of a compound in this article is not limited to a single chemical substance, but can also be interpreted as the same type of chemical substances with the same composition or the same properties.
[0043] If not otherwise specified, in this application, polymer refers to the product formed by the polymerization reaction of monomers, often including many polymer aggregates, each polymer is composed of many simple structural units repeatedly connected by covalent bonds, and the monomer is a compound of synthetic polymers. Polymers can include homopolymers, copolymers, prepolymers, etc., and are not limited to this. Homopolymers refer to polymers polymerized from one monomer. Copolymers refer to polymers polymerized from two or more monomers. Copolymers include random copolymers (structures such as -AABABBBAAABBA-), alternating copolymers (structures such as -ABABABAB-), graft copolymers (structures such as -AA(A-BBBB)AA(A-BBBB)AAA-) and block copolymers (structures such as -AAAAA-BBBBBB-AAAAA-), etc. For example, the styrene-butadiene copolymer in this application can include styrene-butadiene random copolymers, styrene-butadiene alternating copolymers, styrene-butadiene graft copolymers or styrene-butadiene block copolymers when interpreted. Prepolymer refers to a polymer with a lower molecular weight between the monomer and the final polymer, and the prepolymer contains reactive functional groups that can further undergo polymerization to obtain a fully cross-linked or hardened product with a higher molecular weight. Polymers of course include oligomers, but are not limited to them. Oligomers, also known as low polymers, are polymers composed of 2 to 20 repeating units, usually 2 to 5 repeating units.
[0044] For those skilled in the art, a resin composition containing three compounds A, B and C and an additive (comprising four components in total), and a resin composition containing a prepolymer formed by three compounds A, B and C and an additive (comprising two components in total) are different resin compositions, and the two are completely different in many aspects such as the preparation method, the physical and chemical properties of the compounds themselves, and the properties of their products. For example, the former is to mix A, B, C and additives to form a resin composition, while the latter is to first prepolymerize the mixture including A, B and C under appropriate conditions to form a prepolymer, and then mix the prepolymer with the additive to obtain a resin composition. For example, for those skilled in the art, the above two resin compositions have completely different compositions, and because the function of the prepolymer formed by the three compounds A, B and C in the resin composition is completely different from the function of A, B and C individually or together in the resin composition, the two resin compositions should be regarded as completely different chemical substances with completely different chemical positions. For example, for those skilled in the art, because the above two resin compositions are completely different chemical substances, their products will not have the same properties. For example, a resin composition including a prepolymer formed by three compounds A, B and C and a crosslinking agent, since A, B and C have partially reacted or converted during the prepolymerization reaction to form the prepolymer, when the resin composition is subsequently heated at a high temperature to form a semi-cured state, a partial crosslinking reaction occurs between the prepolymer and the crosslinking agent, rather than A, B and C each undergoing a partial crosslinking reaction with the crosslinking agent. Therefore, the products formed by the two resin compositions will also be completely different and have completely different properties.
[0045] Unless otherwise specified, the "resin" in this application is a customary name for a synthetic polymer, which may include monomers, polymers thereof, combinations of monomers, combinations of polymers thereof, or combinations of monomers and polymers thereof, and is not limited thereto.
[0046] If not otherwise specified, in the present application, modified products include products after modification of reactive functional groups of each resin, products after prepolymerization of each resin with other resins, products after crosslinking of each resin with other resins, products after copolymerization of each resin with other resins, etc.
[0047] Unless otherwise specified, the unsaturated bonds described in the present application refer to reactive unsaturated bonds, such as but not limited to unsaturated double bonds that can undergo cross-linking reactions with other functional groups, such as but not limited to unsaturated carbon-carbon double bonds that can undergo cross-linking reactions with other functional groups.
[0048] The unsaturated carbon-carbon double bonds described in the present application preferably include, but are not limited to, vinyl, vinylbenzyl, (meth)acryloyl, allyl or a combination thereof. Vinyl should be interpreted to include vinyl and vinylidene. (Meth)acryloyl should be interpreted to include acryloyl and methacryloyl.
[0049] Unless otherwise specified, the alkyl, alkenyl, and monomer described in this application include their various isomers when interpreted. For example, propyl should be interpreted as including n-propyl and isopropyl.
[0050] Unless otherwise specified, in this application, parts by weight represent relative parts by weight in the composition, which may be any weight unit, such as but not limited to kilograms, kilograms, grams, pounds, etc. For example, 100 parts by weight of polyphenylene ether resin containing unsaturated carbon-carbon double bonds may represent 100 kilograms of polyphenylene ether resin containing unsaturated carbon-carbon double bonds or 100 pounds of polyphenylene ether resin containing unsaturated carbon-carbon double bonds.
[0051] Unless otherwise specified, in the present application, wt% represents weight (or mass) percentage.
[0052] It should be understood that the features disclosed in each implementation scheme herein may be arbitrarily combined to form the technical solution of the present application, as long as there is no contradiction in the combination of these features.
[0053] The present application will be described below with specific embodiments and examples. It should be understood that these specific embodiments and examples are merely exemplary and are not intended to limit the scope of the present application and its use. The methods, reagents and conditions used in the examples are, unless otherwise stated, conventional methods, reagents and conditions in the art.
[0054] As mentioned above, the present invention discloses a resin composition, which includes the following components or prepolymers thereof:
[0055] (A) 100 parts by weight of a polyphenylene ether resin containing unsaturated carbon-carbon double bonds; and
[0056] (B) 10 to 50 parts by weight of a compound of formula (1), wherein the pH value of the compound of formula (1) is 5 to 10;
[0057]
[0058] In formula (1), n is an integer of 3 to 6, and X and Y are each independently o-vinylphenoxy or p-vinylphenoxy, and X and Y are not both o-vinylphenoxy and p-vinylphenoxy;
[0059] The prepolymer is obtained by prepolymerization of a mixture, wherein the mixture includes the component (A) and the component (B).
[0060] For example, in one embodiment, relative to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the resin composition of the present invention includes 10 to 50 parts by weight of the compound of formula (1) (whose pH value is 5 to 10), for example, including but not limited to 10 parts by weight, 15 parts by weight, 20 parts by weight, 25 parts by weight, 30 parts by weight, 35 parts by weight, 40 parts by weight, 45 parts by weight or 50 parts by weight of the compound of formula (1) (whose pH value is 5 to 10).
[0061] For example, in another embodiment, the resin composition includes a prepolymer, which is formed by prepolymerizing 100 parts by weight of a polyphenylene ether resin containing unsaturated carbon-carbon double bonds with 10 to 50 parts by weight of a compound of formula (1) (whose pH value is 5 to 10).
[0062] The prepolymer of the present invention contains residual unsaturated carbon-carbon double bonds, and the conversion rate of the reaction raw materials and the molecular weight of the prepolymer are both within a controllable range.
[0063] For example, in one embodiment, the unsaturated carbon-carbon double bonds remaining in the prepolymer can react with other components (such as a cross-linking agent containing unsaturated carbon-carbon double bonds in the resin composition described below), such as a polymerization reaction or a cross-linking reaction. In the present invention, the presence and content of the unsaturated carbon-carbon double bonds remaining in the prepolymer are controlled by controlling the conversion rate of the compound of formula (1) and the polyphenylene ether resin containing unsaturated carbon-carbon double bonds. The conversion rate of the compound of formula (1) and the polyphenylene ether resin containing unsaturated carbon-carbon double bonds is controlled by means known in the art, such as a hardening accelerator and / or a molecular weight regulator, as well as reaction temperature and reaction time. For example, the conversion rate of the compound of formula (1) may be between 10% and 99%, preferably between 30% and 95%, between 50% and 95%, between 50% and 90%, or between 75% and 90%. For example, when the conversion rate of the compound of formula (1) is 0%, it means that the compound of formula (1) has not reacted at all and the prepolymer of the present invention cannot be formed; when the conversion rate of the compound of formula (1) is 100%, it means that the compound of formula (1) has reacted completely and the prepolymer of the present invention cannot be formed at this time.
[0064] For example, the prepolymer disclosed in the present invention can be prepared by the following method: a mixture of at least 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds and 10 to 50 parts by weight of the compound of formula (1) (whose pH value is 5 to 10) is subjected to prepolymerization under appropriate conditions. For example, the prepolymerization reaction can be carried out in the presence of a hardening accelerator and / or a molecular weight regulator. The types of hardening accelerators are described in detail later. In one or more embodiments, the molecular weight regulator includes: n-butyl mercaptan, dodecyl mercaptan, thioglycolic acid, mercaptopropionic acid, mercaptoethanol, 2,4-diphenyl-4-methyl-1-pentene, 4,4'-butylenebis(6-tert-butyl-3-methylphenol), 2,2'-methylenebis(4-ethyl-6-tert-butylphenol) or a combination thereof.
[0065] The amount of the hardening accelerator and / or molecular weight regulator suitable for the present invention is not particularly limited, and can be 0.01 to 5 parts by weight, for example, 0.1 to 3 parts by weight, respectively, relative to 100 parts by weight of the total amount of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds and the compound of formula (1), and is not limited thereto. Usually, the polyphenylene ether resin containing unsaturated carbon-carbon double bonds and the compound of formula (1) (whose pH value is 5 to 10) and the optional hardening accelerator and / or molecular weight regulator are dissolved in a solvent for prepolymerization. The solvent can be a solvent conventionally used in the art for the polymerization reaction between the monomer or oligomer containing unsaturated carbon-carbon double bonds and the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, including but not limited to toluene and / or butanone. The temperature of the prepolymerization reaction is usually higher than room temperature, for example, between 50°C and 140°C, preferably between 80°C and 120°C. The reaction time is usually 0.5 to 6 hours, preferably 1 to 4 hours. The reaction is usually carried out under stirring conditions. Usually, before the reaction starts, the reaction temperature is first raised to above room temperature. After a period of reaction, the temperature is lowered to room temperature (about 25° C.) to obtain a solution, and a filter is used to filter out impurities in the solution. After the solution is purified, a prepolymer product is obtained, i.e., a prepolymer obtained by prepolymerizing the compound of formula (1) (whose pH value is 5 to 10) with a polyphenylene ether resin containing unsaturated carbon-carbon double bonds.
[0066] The polyphenylene ether resin containing unsaturated carbon-carbon double bonds suitable for use in the present application is not particularly limited, and may be any one or more polyphenylene ether resins containing unsaturated carbon-carbon double bonds suitable for preparing prepregs, resin films, laminates or printed circuit boards, and may be any one or more commercially available products, homemade products or combinations thereof, including, for example, but not limited to, vinylbenzyl polyphenylene ether resins, (meth)acryl polyphenylene ether resins, vinyl polyphenylene ether resins or combinations thereof.
[0067] The polyphenylene ether resin containing unsaturated carbon-carbon double bonds of the present application all have unsaturated carbon-carbon double bonds and a phenylene ether skeleton, wherein the unsaturated carbon-carbon double bonds are reactive functional groups, which can self-polymerize after being heated, and can also undergo free radical polymerization with other unsaturated bond components in the resin composition and finally cross-link and cure. The cured product has the characteristics of high heat resistance and low dielectric. Preferably, the polyphenylene ether resin containing unsaturated carbon-carbon double bonds includes a polyphenylene ether resin containing unsaturated carbon-carbon double bonds substituted with 2,6-dimethyl on the phenylene ether skeleton, and the methyl groups after substitution form a steric hindrance so that the oxygen atoms on the ether are not easy to produce hydrogen bonds or van der Waals forces and absorb moisture, thereby having lower dielectric properties.
[0068] For example, in one embodiment, the polyphenylene ether resin containing unsaturated carbon-carbon double bonds includes, but is not limited to, vinylbenzyl polyphenylene ether resin with a number average molecular weight of about 1200 (e.g., OPE-2st 1200, available from Mitsubishi Gas Chemical Co., Ltd.), vinylbenzyl polyphenylene ether resin with a number average molecular weight of about 2200 (e.g., OPE-2st 2200, available from Mitsubishi Gas Chemical Co., Ltd.), vinylbenzyl polyphenylene ether resin with a number average molecular weight of about 2400 to 2800 (e.g., vinylbenzyl bisphenol A polyphenylene ether resin), (meth)acryl polyphenylene ether resin with a number average molecular weight of about 1900 to 2300 (e.g., SA9000, available from Sabic), vinyl polyphenylene ether resin with a number average molecular weight of about 2200 to 3000, or a combination thereof. The vinyl polyphenylene ether resin may include various types of polyphenylene ether resins disclosed in U.S. Patent Application US20160185904A1, all of which are incorporated herein by reference. For example, in one embodiment, the vinylbenzyl polyphenylene ether resin includes, but is not limited to, vinylbenzyl biphenyl polyphenylene ether resin, vinylbenzyl bisphenol A polyphenylene ether resin, or a combination thereof.
[0069] In the present invention, the compound of formula (1) is a cyclic phosphazene compound containing a P=N bond in its structure, wherein n represents the number of P=N bonds, and n is an integer from 3 to 6. In other words, when n is 3, the compound of formula (1) has a six-membered ring cyclic phosphazene structure, and when n is 6, the compound of formula (1) has a twelve-membered ring cyclic phosphazene structure. In addition, the phosphorus atom in the cyclic phosphazene structure of the compound of formula (1) is substituted by an o-vinylphenoxy group or a p-vinylphenoxy group.
[0070] o-Vinylphenoxy:
[0071] p-Vinylphenoxy:
[0072] In the present invention, for example, when n is 3, the number of o-vinylphenoxy groups in the cyclic phosphazene structure of the compound of formula (1) may be 1, 2, 3, 4 or 5, and the number of p-vinylphenoxy groups may be 5, 4, 3, 2 or 1. When n is 6, the number of o-vinylphenoxy groups in the cyclic phosphazene structure of the compound of formula (1) may be 1, 2, 3, 4, 5, 6, 7, 8, 9, 10 or 11, and the number of p-vinylphenoxy groups may be 11, 10, 9, 8, 7, 6, 5, 4, 3, 2 or 1.
[0073] The pH value of the compound of formula (1) is 5 to 10. In the present invention, unless otherwise specified, the pH value of the compound can be measured by a measuring instrument known in the art, such as but not limited to measurement using a pH meter, or for example, titration using an acid-base titration method. For example, in one embodiment, the compound of formula (1) and deionized water with a pH value of 7 are mixed in a weight ratio of 1:10, the mixed solution is filtered and extracted at room temperature, and the pH value of the extract is measured using a pH meter to obtain the pH value of the compound of formula (1). For example, in one embodiment, the pH value of the compound of formula (1) may be 5 to 10, such as but not limited to, the pH value of the compound of formula (1) may be 5, 6, 7, 8, 9 or 10. When measured by a pH meter, the pH value of the compound of formula (1) may also be a small value, such as but not limited to 5.5, 6.5 or 7.3, and is not limited thereto.
[0074] The compound of formula (1) described in the present application can be prepared by various methods known to those skilled in the art. For example, the compound of formula (1) can be prepared by the following method:
[0075] Step (1), reacting cyclophosphazene with o-hydroxybenzaldehyde to obtain an intermediate product 1;
[0076] Step (2), reacting the intermediate product 1 with p-hydroxybenzaldehyde to obtain the intermediate product 2;
[0077] Step (3), reacting the intermediate product 2 with methyltriphenylphosphonium bromide in the presence of a catalytic base to obtain a compound of formula (1).
[0078] In step (1), a base may be further added, including but not limited to an acid binding agent, potassium carbonate, triethylamine or a combination thereof.
[0079] In step (1), an organic solvent may be further added, including but not limited to tetrahydrofuran. Unless otherwise specified, the tetrahydrofuran used in the present invention is tetrahydrofuran from which water has been removed (anhydrous tetrahydrofuran).
[0080] In step (1), the cyclophosphazene includes but is not limited to hexachlorocyclotriphosphazene, octachlorocyclotetraphosphazene, decachlorocyclopentaphosphazene, and dodecachlorocyclohexaphosphazene. The molar ratio of the cyclophosphazene to o-hydroxybenzaldehyde is 1:1 to 1:11.
[0081] The reaction temperature of step (1) is 40 to 80° C., and the reaction time is 24 to 96 hours.
[0082] In step (2), the molar amount of p-hydroxybenzaldehyde added is 1 to 11 times the molar amount of cyclophosphazene added in step (1), that is, the molar ratio of cyclophosphazene to p-hydroxybenzaldehyde added is 1:1 to 1:11.
[0083] The reaction temperature of step (2) is 40 to 80° C., and the reaction time is 24 to 96 hours.
[0084] In step (3), an organic solvent from which water has been removed may be further added, including but not limited to tetrahydrofuran from which water has been removed.
[0085] In step (3), the catalytic base includes but is not limited to potassium tert-butoxide, sodium methoxide or a combination thereof.
[0086] In step (3), the pH value of the reaction system is adjusted to 3 to 13 by using an acetic acid aqueous solution or an ammonium chloride aqueous solution.
[0087] The reaction temperature of step (3) is 25 to 50° C., and the reaction time is 1 to 6 hours.
[0088] For example, in one embodiment, the resin composition may further include polyolefin. For example, in the resin composition of the present invention, the amount of polyolefin is not particularly limited relative to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, and may be 5 to 25 parts by weight, including but not limited to 5 parts by weight, 10 parts by weight, 15 parts by weight, 20 parts by weight or 25 parts by weight.
[0089] The polyolefin applicable to the present application is not particularly limited, and may be any one or more polyolefins applicable to the preparation of prepregs, resin films, laminates or printed circuit boards, and may be any one or more commercially available products, homemade products or combinations thereof. For example, the polyolefin applicable to the present application includes but is not limited to diene polymers, monoene polymers, hydrogenated diene polymers or combinations thereof. The diene is a hydrocarbon compound containing two unsaturated carbon-carbon double bonds in the molecule, and the monoene is a hydrocarbon compound containing one unsaturated carbon-carbon double bond in the molecule. Suitable polyolefins for the present application include, for example, but are not limited to, any one of polybutadiene, polyisoprene, styrene-butadiene copolymer, styrene-isoprene copolymer, styrene-butadiene-divinylbenzene terpolymer, styrene-butadiene-maleic anhydride terpolymer, vinyl-polybutadiene-urea polymer, maleic anhydride-butadiene copolymer, polymethylstyrene, hydrogenated polybutadiene, hydrogenated polyisoprene, hydrogenated styrene-butadiene-divinylbenzene terpolymer, hydrogenated styrene-butadiene-maleic anhydride terpolymer, hydrogenated styrene-butadiene copolymer, hydrogenated styrene-isoprene copolymer, and multifunctional vinyl aromatic copolymers or any combination thereof.
[0090] For example, if not specifically stated, the multifunctional vinyl aromatic copolymer used in the present invention may include various types of multifunctional vinyl aromatic copolymers disclosed in US Pat. No. 20070129502A1, which are all incorporated herein by reference.
[0091] For example, in one embodiment, the resin composition of the present invention may further include a cross-linking agent containing unsaturated carbon-carbon double bonds. Relative to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the resin composition of the present invention contains 2 to 10 parts by weight of the cross-linking agent containing unsaturated carbon-carbon double bonds.
[0092] The cross-linking agent containing unsaturated carbon-carbon double bonds applicable to the present application refers to a small molecule compound containing unsaturated carbon-carbon double bonds with a molecular weight less than or equal to 1000, and the molecular weight is preferably between 100 and 900, and more preferably between 100 and 800. For example, the cross-linking agent containing unsaturated carbon-carbon double bonds is any one of bis(vinylphenyl)ethane (BVPE), divinylbenzene (DVB), divinylnaphthalene, divinylbiphenyl, tert-butylstyrene, triallyl isocyanurate (TAIC), triallyl cyanurate (TAC), vinylbenzocyclobutene (VBCB), di(vinylbenzyl)ether (bis(vinylbenzyl)ether, BVBE), trivinylcyclohexane (TVCH), diallyl isophthalate (DAIP), diallyl bisphenol A (DABPA), acrylate, butadiene, decadiene, octadiene, vinyl carbazole, styrene, or a combination thereof.
[0093] For example, in one embodiment, the resin composition may further contain any one or a combination of epoxy resin, polyester resin, phenol resin, amine curing agent, polyamide, polyimide, styrene maleic anhydride, and cyanate ester as needed.
[0094] In the present invention, for example, the epoxy resin can be any epoxy resin known in the art. From the perspective of improving the heat resistance of the resin composition, the epoxy resin includes, but is not limited to, for example, bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, bisphenol AD epoxy resin, novolac epoxy resin, trifunctional epoxy resin, tetrafunctional epoxy resin, multifunctional novolac epoxy resin, dicyclopentadiene (DCPD) epoxy resin, phosphorus-containing epoxy resin, p-xylene epoxy resin, naphthalene epoxy resin (e.g., naphthol epoxy resin), benzofuran epoxy resin, isocyanate-modified epoxy resin, any one or a combination thereof. In the present invention, for example, the novolac epoxy resin may be phenol novolac epoxy resin, bisphenol A novolac epoxy resin, bisphenol F novolac epoxy resin, biphenyl novolac epoxy resin, phenol benzaldehyde epoxy resin, phenol aralkyl novolac epoxy resin or o-cresol novolac epoxy resin. In the present invention, for example, the phosphorus-containing epoxy resin may be DOPO (9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide) epoxy resin, DOPO-HQ epoxy resin or a combination thereof.The DOPO epoxy resin may be selected from one or more of DOPO-containing phenol novolac epoxy resin, DOPO-containing o-cresol novolac epoxy resin and DOPO-containing bisphenol-A novolac epoxy resin; the DOPO-HQ epoxy resin may be selected from one or more of DOPO-HQ-containing phenol novolacepoxy resin, DOPO-HQ-containing o-cresol novolac epoxy resin and DOPO-HQ-containing bisphenol-A novolac epoxy resin, but is not limited thereto.
[0095] If not otherwise specified, the amount of epoxy resin used in the present invention can be adjusted as needed, for example, including but not limited to, relative to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the amount of epoxy resin can be 10 to 100 parts by weight, for example, 10 parts by weight, 15 parts by weight, 20 parts by weight, 30 parts by weight, 40 parts by weight, 50 parts by weight, 60 parts by weight, 70 parts by weight, 80 parts by weight, 90 parts by weight or 100 parts by weight.
[0096] In the present invention, for example, the polyester resin can be various polyester resins known in the art. Specific examples include, but are not limited to, polyester resins containing dicyclopentadiene structures and polyester resins containing naphthalene ring structures. Specific examples include, but are not limited to, the trade names HPC-8000 or HPC-8150 sold by Dainippon Ink Chemical. If not otherwise specified, the amount of the polyester resin used in the present invention can be adjusted as needed, for example, including but not limited to, relative to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the amount of the polyester resin can be 10 to 80 parts by weight, such as 10 parts by weight, 15 parts by weight, 20 parts by weight, 30 parts by weight, 40 parts by weight, 50 parts by weight, 60 parts by weight, 70 parts by weight or 80 parts by weight.
[0097] In the present invention, for example, the phenol resin can be various phenol resins known in the art, and specific examples include but are not limited to phenolic resins or phenoxy resins, wherein the phenolic resin includes phenolic resin, o-methylphenolic resin, bisphenol A resin, naphthol resin, biphenyl resin and dicyclopentadiene phenol resin, and is not limited thereto. If not specifically indicated, the amount of the phenolic resin used in the present invention can be adjusted as needed, for example, including but not limited to, relative to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the amount of the phenolic resin can be 10 to 80 parts by weight, such as 10 parts by weight, 15 parts by weight, 20 parts by weight, 30 parts by weight, 40 parts by weight, 50 parts by weight, 60 parts by weight, 70 parts by weight or 80 parts by weight.
[0098] In the present invention, for example, the amine curing agent can be various amine curing agents known in the art. Specific examples include but are not limited to at least one of diaminodiphenyl sulfone, diaminodiphenylmethane, diaminodiphenyl ether, diaminodiphenyl sulfide and dicyandiamide or a combination thereof. If not specifically stated, the amount of the amine curing agent used in the present invention can be adjusted as needed, for example, including but not limited to, relative to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the amount of the amine curing agent can be 1 to 15 parts by weight, for example, 1 part by weight, 4 parts by weight, 7.5 parts by weight, 12 parts by weight or 15 parts by weight.
[0099] In the present invention, for example, the polyamide may be various polyamides known in the art, including but not limited to various commercially available polyamide resin products.
[0100] In the present invention, for example, the polyimide may be various polyimides known in the art, including but not limited to various commercially available polyimide resin products.
[0101] In the present invention, for example, styrene maleic anhydride can be various types of styrene maleic anhydride known in the art, wherein the ratio of styrene (St) to maleic anhydride (MA) can be 1 / 1, 2 / 1, 3 / 1, 4 / 1, 6 / 1, 8 / 1 or 12 / 1. Specific examples include styrene maleic anhydride copolymers sold by Cray Valley under the trade names of SMA-1000, SMA-2000, SMA-3000, EF-30, EF-40, EF-60 and EF-80, or styrene maleic anhydride copolymers sold by Polyscope under the trade names of C400, C500, C700, C900, and the like, and are not limited thereto.
[0102] In the present invention, for example, the cyanate ester may be any one or more cyanate ester resins suitable for preparing a prepreg, a resin film, a laminate or a printed circuit board, such as a compound having an Ar-OC≡N structure, wherein Ar may be a substituted or unsubstituted aromatic group. From the perspective of improving the heat resistance of the resin composition, specific examples of cyanate ester resins include, but are not limited to, phenolic cyanate ester resins, bisphenol A cyanate ester resins, bisphenol F cyanate ester resins, cyanate ester resins containing a dicyclopentadiene structure, cyanate ester resins containing a naphthalene ring structure, phenolphthalein cyanate ester resins, adamantane cyanate ester resins, fluorene cyanate ester resins or combinations thereof. Among them, the phenolic cyanate ester resin may be a bisphenol A phenolic cyanate ester resin, a bisphenol F phenolic cyanate ester resin or a combination thereof. For example, the cyanate resin may be a cyanate resin produced by Lonza under the trade names of Primaset PT-15, PT-30S, PT-60S, BA-200, BA-230S, BA-3000S, BTP-2500, BTP-6020S, DT-4000, DT-7000, ULL950S, HTL-300, CE-320, LVT-50, LeCy, etc.
[0103] For example, in some embodiments, the resin composition may further include any one or a combination of inorganic fillers, flame retardants, hardening accelerators, polymerization inhibitors, solvents, silane coupling agents, colorants, and toughening agents as needed.
[0104] In the present invention, for example, the inorganic filler can be any one or more inorganic fillers suitable for preparing prepregs, resin films, laminates or printed circuit boards, and specific examples thereof include, but are not limited to, silicon dioxide (molten, non-molten, porous or hollow), aluminum oxide, aluminum hydroxide, magnesium oxide, magnesium hydroxide, calcium carbonate, aluminum nitride, boron nitride, aluminum silicon carbide, silicon carbide, titanium dioxide, barium titanate, lead titanate, strontium titanate, calcium titanate, magnesium titanate, barium zirconate, lead zirconate, magnesium zirconate, lead zirconate titanate, zinc molybdate, calcium molybdate, magnesium molybdate, ammonium molybdate, zinc molybdate-modified talc, zinc oxide, zirconium oxide, mica, boehmite (AIOOH), calcined talc, talc, silicon nitride, zirconium tungstate, petalite, calcined kaolin or a combination thereof. In addition, the inorganic filler may be spherical (including solid spherical or hollow spherical), fibrous, plate-like, granular, flaky or needle-like, and may be selectively pretreated with a silane coupling agent. For example, in one embodiment, relative to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the resin composition of the present invention may further include 10 to 200 parts by weight of the inorganic filler, preferably 50 to 150 parts by weight of the inorganic filler, more preferably 80 to 130 parts by weight of the inorganic filler, including but not limited to this.
[0105] For example, the flame retardant applicable to the present invention may be any one or more flame retardants applicable to the preparation of prepregs, resin films, laminates or printed circuit boards, such as but not limited to phosphorus-containing flame retardants or bromine-containing flame retardants. The bromine-containing flame retardant preferably includes decabromodiphenylethane, and the phosphorus-containing flame retardant preferably includes: hydroquinone bis-(diphenyl phosphate), bisphenol A bis-(diphenyl phosphate), tris(2-carboxyethyl)phosphine (tfi(2-carboxyethyl)phosphine, TCEP), tris(chloroisopropyl) phosphate, trimethyl phosphate (trimethyl phosphate, TMP), dimethyl methylphosphonate (dimethylmethyl phosphonate, DMMP), resorcinol bis(dixylenylphosphate), RDXP (such as PX-200, PX-201, PX-202 and other commercial products)), ammonium polyphosphate, melamine polyphosphate, etc. polyphosphate), DPPO (diphenylphosphineoxide) and its derivatives (such as bis-DPPO compounds) or resins, melamine cyanurate and tri-hydroxyethylisocyanurate, aluminum phosphinate (such as OP-930, OP-935 and other products) or combinations thereof.
[0106] For example, in one embodiment, the flame retardant can also be a flame retardant sold by Katayama Chemical Industry Co., Ltd., such as but not limited to V1, V2, V3, V4, V5, V7, S-2, S-4, E-4c, E-7c, E-8g, E-9g, E-10g, E-100, B-3, W-1o, W-2h, W-2o, W-3o, W-4o, OX-1, OX-2, OX-4, OX-6, OX-6+, OX-7, OX-7+, OX-13, BPE-1, BPE-3, HyP-2, API-9, CMPO, ME-20, C-1R, C-1S, C-3R, C-3S or C-11R. The flame retardant of the present invention can include one or more of the above.
[0107] The present invention preferably includes a phosphate flame retardant, for example including but not limited to resorcinol bis-(xylyl phosphate) or its polycondensate, a phosphate containing an unsaturated carbon-carbon double bond or a combination thereof.
[0108] The phosphate containing unsaturated carbon-carbon double bonds of the present invention includes the structure shown in P1,
[0109]
[0110] Wherein, A is independently a C1-C3 alkyl group, B is a functional group containing an unsaturated carbon-carbon double bond, preferably, B is vinyl, vinylbenzyl, allyl or butadienyl. Specific examples of the phosphate containing an unsaturated carbon-carbon double bond include, but are not limited to, flame retardants sold by Katayama Chemical Industry Co., Ltd. under the trade names of S-2, V2, and B-3.
[0111] For example, in one embodiment, relative to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the resin composition of the present invention may further include 1 to 15 parts by weight of a phosphate flame retardant, preferably 2 to 10 parts by weight of a phosphate flame retardant, including but not limited to.
[0112] For example, in one embodiment, the weight ratio of the compound of formula (1) to the phosphate flame retardant is between 25:1 and 1.5:1. For example, but not limited to, the weight ratio of the compound of formula (1) to the phosphate flame retardant is 25:1, 20:1, 15:1, 10:1, 9:1, 8:1, 7:1, 6.5:1, 6.25:1, 6:1, 5:1, 4:1, 3:1, 2.5:1, 2:1 or 1.5:1.
[0113] For example, the hardening accelerator (including the hardening initiator) may include a catalyst such as a Lewis base or a Lewis acid. The Lewis base may include one or more of imidazole, boron trifluoride amine complex, ethyltriphenyl phosphonium chloride, 2-methylimidazole (2MI), 2-phenyl-1H-imidazole (2PZ), 2-ethyl-4-methylimidazole (2E4MI), triphenylphosphine (TPP) and 4-dimethylaminopyridine (DMAP). The Lewis acid may include a metal salt compound such as a metal salt compound of manganese, iron, cobalt, nickel, copper, zinc, etc., such as a metal catalyst such as zinc octoate and cobalt octoate. The hardening accelerator also includes a hardening initiator, such as a peroxide that can generate free radicals, and the hardening initiator includes but is not limited to: diisopropylbenzene peroxide, tert-butyl peroxybenzoate, dibenzoyl peroxide (BPO), 2,5-dimethyl-2,5-di(tert-butylperoxy)-3-hexyne (25B) and bis(tert-butylperoxyisopropyl)benzene or a combination thereof. For example, in one embodiment, relative to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the resin composition of the present invention may further include 0.001 to 2 parts by weight of a hardening accelerator, preferably 0.01 to 1.5 parts by weight of a hardening accelerator, and more preferably 0.1 to 1.0 parts by weight of a hardening accelerator, including but not limited to this.
[0114] For example, the inhibitor may include, but is not limited to, 1,1-diphenyl-2-trinitrophenylhydrazine, methacrylonitrile, nitrogen oxide stable free radicals, triphenylmethyl free radicals, metal ion free radicals, sulfur free radicals (for example, but not limited to dithioesters), hydroquinone, p-methoxyphenol, p-benzoquinone, phenothiazine, β-phenylnaphthylamine, p-tert-butylcatechol, methylene blue, 4,4'-butylenebis(6-tert-butyl-3-methylphenol) and 2,2'-methylenebis(4-ethyl-6-tert-butylphenol) or a combination thereof. For example, the above-mentioned nitrogen oxide stable free radicals may include, but are not limited to, nitrogen oxide free radicals from cyclic hydroxylamines such as 2,2,6,6-tetramethyl-1-oxy-piperidine, 2,2,6,6-substituted-1-piperidinyloxy free radicals or 2,2,5,5-substituted-1-pyrrolidinyloxy free radicals. As a substituent, an alkyl group with a carbon number of less than four, such as a methyl group or an ethyl group, is preferred. Specific nitrogen oxide free radical compounds are not limited, and examples include but are not limited to 2,2,6,6-tetramethyl-1-piperidinyloxy free radical, 2,2,6,6-tetraethyl-1-piperidinyloxy free radical, 2,2,6,6-tetramethyl-4-oxo-1-piperidinyloxy free radical, 2,2,5,5-tetramethyl-1-pyrrolidinyloxy free radical, 1,1,3,3-tetramethyl-2-isoindolinyloxy free radical, N,N-di-tert-butylamineoxy free radical, etc. Stable free radicals such as galvinoxyl free radical can also be used to replace the nitrogen oxide free radical. The inhibitor suitable for the resin composition of the present invention can also be a product derived from the hydrogen atom or atomic group in the inhibitor replaced by other atoms or atomic groups. For example, the hydrogen atom in the inhibitor is replaced by atomic groups such as amino, hydroxyl, ketocarbonyl and the like and derived products. For example, in one embodiment, relative to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the resin composition of the present invention may further include 0.001 to 20 parts by weight of a polymerization inhibitor, preferably 0.001 to 10 parts by weight of a polymerization inhibitor, including but not limited to this.
[0115] For example, the solvent suitable for the resin composition of the present invention is not particularly limited, and can be any solvent suitable for dissolving the resin composition of the present invention, including but not limited to: methanol, ethanol, ethylene glycol monomethyl ether, acetone, butanone (also known as methyl ethyl ketone), methyl isobutyl ketone, cyclohexanone, nitrogen methyl pyrrolidone, toluene, xylene, methoxyethyl acetate, ethoxyethyl acetate, propoxyethyl acetate, ethyl acetate, dimethylformamide, dimethylacetamide, propylene glycol methyl ether acetate and other solvents or mixed solvents thereof. The amount of solvent added is to be able to completely dissolve the resin and adjust to a specific total solid content of the resin composition. For example, in one embodiment, the amount of solvent added is adjusted to a total solid content of 50% to 85% for addition, including but not limited to this.
[0116] For example, the silane coupling agent applicable to the present invention may include silane compounds (silane, for example, including but not limited to siloxane compounds), which can be divided into aminosilane compounds, epoxysilane compounds, vinylsilane compounds, hydroxylsilane compounds, isocyanatesilane compounds, methacryloxysilane compounds and acryloxysilane compounds according to the type of functional group. For example, in one embodiment, relative to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the resin composition of the present invention may further include 0.001 to 20 parts by weight of a silane coupling agent, preferably 0.01 to 10 parts by weight of a silane coupling agent, including but not limited to this.
[0117] For example, coloring agents may include, but are not limited to, dyes or pigments.
[0118] In the present invention, the main function of adding a toughening agent is to improve the toughness of the resin composition. For example, the toughening agent suitable for the present invention may include, but is not limited to, carboxyl-terminated butadieneacrylonitrile rubber (CTBN), core-shell rubber, ethylene-propylene rubber and other compounds or combinations thereof. For example, in one embodiment, relative to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the resin composition of the present invention may further include 1 to 20 parts by weight of a toughening agent, preferably 3 to 10 parts by weight of a toughening agent, but is not limited thereto.
[0119] The present invention also provides a product made of the resin composition, such as a component suitable for various electronic products, including but not limited to: a prepreg, a resin film, a laminate or a printed circuit board.
[0120] For example, the resin composition of the present invention can be made into a semi-cured sheet, which includes a reinforcing material and a layered object arranged on the reinforcing material. The layered object is obtained by heating the aforementioned resin composition at a high temperature to form a semi-cured state (B-stage). The baking temperature for making the semi-cured sheet is between 120°C and 180°C, preferably between 120°C and 160°C. The reinforcing material can be any one of a fiber material, a woven fabric, and a non-woven fabric, and the woven fabric preferably includes a glass fiber cloth. The type of glass fiber cloth is not particularly limited, and can be various glass fiber cloths that can be used for printed circuit boards, such as E-type glass cloth, D-type glass cloth, S-type glass cloth, T-type glass cloth, L-type glass cloth, Q-type glass cloth or QL-type glass cloth (a glass cloth of a mixed structure made of Q glass and L glass); the types of glass fibers include yarns and rovings, etc., and the forms include open fiber or unopen fiber, and the end face shape includes a circular or flat shape. The aforementioned non-woven fabric preferably includes a liquid crystal resin non-woven fabric, such as a polyester non-woven fabric, a polyurethane non-woven fabric, etc., and is not limited thereto. The aforementioned fabric may also include a liquid crystal resin fabric, such as a polyester fabric or a polyurethane fabric, etc., and is not limited thereto. This reinforcing material can increase the mechanical strength of the prepreg. In a preferred embodiment, the reinforcing material can also be selectively pretreated with a silane coupling agent. The prepreg is subsequently heated and cured (C-stage) to form an insulating layer.
[0121] For example, the resin composition of the present invention can be made into a resin film, which is obtained by semi-curing the aforementioned resin composition after baking and heating. The resin composition can be selectively coated on a liquid crystal resin film, a polytetrafluoroethylene film, a polyethylene terephthalate film (PET film), a polyimide film (PI film), a copper foil or a copper foil with adhesive, and then semi-cured by baking and heating to form a resin film.
[0122] For example, the resin composition described in the present application can be made into various laminates, which include at least two metal foils and at least one insulating layer, wherein the insulating layer is disposed between the two metal foils, and the insulating layer can be formed by curing the aforementioned resin composition under high temperature and high pressure (C-stage), and the applicable curing temperature is, for example, between 190°C and 220°C, preferably between 200°C and 210°C, and the curing time is 90 to 180 minutes, preferably 120 to 150 minutes. The aforementioned insulating layer can be obtained by curing the aforementioned semi-cured sheet or resin film. The material of the aforementioned metal foil can be copper, aluminum, nickel, platinum, silver, gold or their alloys, such as copper foil. In a preferred embodiment, the laminate is a copper foil substrate.
[0123] In one embodiment, the aforementioned laminate can be further processed into a printed circuit board. One of the methods for making the printed circuit board of the present application can be to use a double-sided copper-clad laminate (for example, product EM-827, which can be purchased from Taiwan Optoelectronics Materials) with a thickness of 28 mils and 1 ounce of HTE (High Temperature Elongation) copper foil, and electroplating after drilling to form electrical conduction between the upper copper foil and the bottom copper foil. The upper copper foil and the bottom copper foil are then etched to form an inner layer circuit. The inner layer circuit is then browned and roughened to form a concave-convex structure on the surface to increase the roughness. Then, the copper foil, the aforementioned prepreg, the aforementioned inner layer circuit board, the aforementioned prepreg, and the copper foil are stacked in sequence, and then a vacuum laminating device is used to heat for 90 to 180 minutes at a temperature of 190°C to 220°C to cure the insulating layer material of the prepreg. Next, various circuit board processing techniques known in the art such as blackening, drilling, and copper plating are performed on the copper foil on the outermost surface to obtain a printed circuit board.
[0124] For example, in one or more embodiments, the resin composition disclosed in the present application and various products prepared therefrom preferably have one or more of the following characteristics:
[0125] There is no shadow on the copper-free surface of the inner circuit substrate without copper on the surface;
[0126] The adhesion between the resin and glass fiber interface in the substrate was observed to be acceptable using a scanning electron microscope;
[0127] The resistance value change rate after 1000 cycles of interconnect stress test measured according to IPC-TM-650 2.6.26 is less than 10% (the product passes the interconnect stress test);
[0128] The interlayer bonding strength measured according to the method of IPC-TM-650 2.4.8 is greater than or equal to 3.5 lb / in, such as between 3.5 lb / in and 4.5 lb / in;
[0129] The dielectric constant temperature coefficient measured according to the method of IPC-TM-650 2.5.5.13 is less than or equal to 73 ppm / °C, for example, between 37 ppm / °C and 73 ppm / °C;
[0130] The dielectric loss temperature coefficient measured according to the method of IPC-TM-650 2.5.5.13 is less than or equal to 6300 ppm / °C, for example, between 2939 ppm / °C and 6215 ppm / °C;
[0131] After the product is left to stand for 500 hours at a temperature of 85° C. and a relative humidity of 85%, the dielectric loss aging rate calculated by measuring the dielectric loss at a frequency of 10 GHz according to the JIS C2565 method is less than or equal to 57%, for example, between 23% and 57%.
[0132] The resin compositions of the embodiments and comparative examples of the present invention were prepared using various raw materials from the following sources and in the amounts shown in Tables 1 to 5, and were further made into various test samples.
[0133] The chemical raw materials used in the embodiments of the present invention and the comparative examples are as follows:
[0134] SA9000: (meth)acryl polyphenylene ether resin, available from Sabic.
[0135] OPE-2st 2200: vinyl benzyl polyphenylene ether resin, purchased from Mitsubishi Gas Chemical.
[0136] OPE-2st1200: vinyl benzyl polyphenylene ether resin, purchased from Mitsubishi Gas Chemical.
[0137] Compounds A1-A8 and C1-C6 were prepared in-house and are described in detail below.
[0138] G1726: hydrogenated styrene-butadiene-styrene triblock copolymer (SEBS), available from Kraton Corporation.
[0139] B-3000: polybutadiene, purchased from Nippon Soda.
[0140] Ricon 100: Styrene-butadiene copolymer, available from Cray Valley.
[0141] Ricon 184MA6: styrene-butadiene-maleic anhydride terpolymer, available from Cray Valley Corporation.
[0142] SPV-100: Allylphosphazene, purchased from Otsuka Chemical.
[0143] Di-DOPO: di-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, the structure of which is shown in formula (2).
[0144]
[0145] PX-200: Resorcinol bis-(xylyl phosphate) (condensation polymer), or 1,3-phenylene phosphate tetrakis (2,6-dimethylphenyl) ester (condensation polymer), purchased from Daihachi Chemical of Japan.
[0146] S-2: diethyl p-vinylbenzyl phosphate, purchased from Katayama Chemical Co., Ltd.
[0147] DVB: divinylbenzene, purchased from Shanghai MacLean Biochemical Technology Co., Ltd.
[0148] TAIC: triallyl isocyanurate, purchased from Chin Yu Enterprise Co., Ltd.
[0149] SC-2500 SVJ: spherical silica with surface treated with silane coupling agent, purchased from Admatechs.
[0150] 25B: 2,5-dimethyl-2,5-di(tert-butylperoxy)-3-hexyne, purchased from NOF Corporation.
[0151] Toluene: purchased from Sinopec. The toluene content is expressed as "appropriate amount", which means that the toluene content is adjusted to a solid content of 60% to 68% (solid content, S / C = 60% to 68%) of the resin composition.
[0152] Homemade compound A1:
[0153] At room temperature, 100 g of hexachlorocyclotriphosphazene, 270 g of potassium carbonate and 400 ml of tetrahydrofuran were added to a three-necked flask. After sufficient dissolution, the three-necked flask was moved to an ice-water bath. 37 g of o-hydroxybenzaldehyde was slowly added dropwise to the three-necked flask. After 2 hours of dropwise addition, the temperature was raised to 40°C and the reaction was continued for 72 hours. Then, 366 ml of a tetrahydrofuran solution of p-hydroxybenzaldehyde with a concentration of 0.5 g / ml was added dropwise to the three-necked flask, the reaction was continued for 48 hours, and the intermediate was obtained by filtering and rotary evaporation.
[0154] At room temperature, 315 g of dehydrated methyltriphenylphosphonium bromide and 500 ml of a dehydrated tetrahydrofuran solution of an intermediate with a concentration of 0.17 g / ml were added to a three-necked flask, stirred, and 100 g of freshly unsealed potassium tert-butoxide was slowly added. After reacting for 2 hours, 600 g of calcium bromide was added, and the reaction was stirred for 24 hours. An acetic acid aqueous solution was added to adjust the pH value to 4.5 to 5, and tetrahydrofuran in the system was removed by rotary evaporation. Ethyl acetate was added, and the liquids were separated and the oil phase was collected. After the ethyl acetate was removed by rotary evaporation, a mixed solution of cyclohexane and ethyl acetate was used as a mobile phase (cyclohexane: ethyl acetate = 500: 1-10: 1), and the product was separated and purified by a silica gel chromatography column to obtain a product labeled A1, with a measured pH of 5. The specific structure is shown in formula (3).
[0155]
[0156] If not otherwise specified, in the present invention, the pH value of a compound is determined as follows: the compound and deionized water with a pH value of 7 are mixed in a weight ratio of 1:10, the mixed solution is filtered and extracted at room temperature, and the pH value of the extract is determined using a pH meter to obtain the pH value of the compound.
[0157] Homemade compound A2:
[0158] At room temperature, 100 g of hexachlorocyclotriphosphazene, 198 g of triethylamine and 400 ml of tetrahydrofuran were added to a three-necked flask. After sufficient dissolution, the three-necked flask was moved to an ice-water bath. 110 g of o-hydroxybenzaldehyde was slowly added dropwise to the three-necked flask. After 2 hours of dropwise addition, the temperature was raised to 50° C. and the reaction was continued for 64 hours. Then, 220 ml of a tetrahydrofuran solution of p-hydroxybenzaldehyde with a concentration of 0.5 g / ml was added dropwise to the three-necked flask. The reaction was continued for 60 hours, filtered and rotary evaporated to obtain an intermediate.
[0159] At room temperature, 350 g of dehydrated methyltriphenylphosphonium bromide and 500 ml of a dehydrated tetrahydrofuran solution of the intermediate with a concentration of 0.17 g / ml were added to a three-necked flask, stirred, and 100 g of freshly unsealed potassium tert-butoxide was slowly added. After reacting for 2 hours, 600 g of calcium bromide was added, and the reaction was stirred for 24 hours. An acetic acid aqueous solution was added to adjust the pH value to 7 to 8, and tetrahydrofuran in the system was removed by rotary evaporation. Ethyl acetate was added, and the liquid was separated. The oil phase was collected. After the ethyl acetate was removed by rotary evaporation, a mixed solution of cyclohexane and ethyl acetate was used as a mobile phase (cyclohexane: ethyl acetate = 500: 1-10: 1), and the product was separated and purified by a silica gel chromatography column to obtain a product labeled A2. The pH value was measured to be 8. The specific structure is shown in formula (4).
[0160]
[0161] Homemade compound A3:
[0162] At room temperature, 100 g of hexachlorocyclotriphosphazene, 270 g of potassium carbonate and 400 ml of tetrahydrofuran were added to a three-necked flask. After sufficient dissolution, the three-necked flask was moved to an ice-water bath. 183 g of o-hydroxybenzaldehyde was slowly added dropwise to the three-necked flask. After 2 hours of dropwise addition, the temperature was raised to 60°C and the reaction was continued for 56 hours. Then, 73 ml of a tetrahydrofuran solution of p-hydroxybenzaldehyde with a concentration of 0.5 g / ml was added dropwise to the three-necked flask. The reaction was continued for 72 hours, filtered and rotary evaporated to obtain an intermediate.
[0163] At room temperature, 400 g of dehydrated methyltriphenylphosphonium bromide and 550 ml of a dehydrated tetrahydrofuran solution of the intermediate with a concentration of 0.17 g / ml were added to a three-necked flask, stirred, and 48 g of newly opened sodium methoxide was slowly added. After reacting for 2 hours, 600 g of calcium bromide was added, and the reaction was stirred for 24 hours. An aqueous ammonium chloride solution was added to adjust the pH value to 9 to 10, and tetrahydrofuran in the system was removed by rotary evaporation. Ethyl acetate was added, and the liquids were separated. The oil phase was collected. After the ethyl acetate was removed by rotary evaporation, a mixed solution of cyclohexane and ethyl acetate was used as a mobile phase (cyclohexane: ethyl acetate = 500: 1-10: 1), and the product was separated and purified by a silica gel chromatography column to obtain a product labeled A3. The pH value was measured to be 10. The specific structure is shown in formula (5).
[0164]
[0165] Homemade compound A4:
[0166] At room temperature, 134 g of octachlorocyclotetraphosphazene, 359 g of potassium carbonate and 400 ml of tetrahydrofuran were added to a three-necked flask. After sufficient dissolution, the three-necked flask was moved to an ice-water bath. 147 g of o-hydroxybenzaldehyde was slowly added dropwise to the three-necked flask. After 2 hours of dropwise addition, the temperature was raised to 70°C and the reaction was continued for 48 hours. Then, 293 ml of a tetrahydrofuran solution of p-hydroxybenzaldehyde with a concentration of 0.5 g / ml was added dropwise to the three-necked flask. The reaction was continued for 48 hours, filtered and rotary evaporated to obtain an intermediate.
[0167] At room temperature, 315 g of dehydrated methyltriphenylphosphonium bromide and 500 ml of dehydrated tetrahydrofuran solution of the intermediate with a concentration of 0.17 g / ml were added to a three-necked flask, stirred, and 135 g of freshly unsealed potassium tert-butoxide were slowly added. After reacting for 3 hours, 700 g of calcium bromide were added, and the reaction was stirred for 48 hours. An acetic acid aqueous solution was added to adjust the pH value to 7 to 8, and tetrahydrofuran in the system was removed by rotary evaporation. Dichloroethane was added, the liquids were separated, and the oil phase was collected. After the dichloroethane was removed by rotary evaporation, a mixed solution of cyclohexane and dichloroethane was used as a mobile phase (cyclohexane: dichloroethane = 500: 1-10: 1), and the product was separated and purified by a silica gel chromatography column to obtain a product labeled A4. The pH value was measured to be 8, and the specific structure is shown in formula (6).
[0168]
[0169] Homemade compound A5:
[0170] At room temperature, 168 g of decachlorocyclopentaphosphazene, 442 g of potassium carbonate and 400 ml of tetrahydrofuran were added to a three-necked flask. After fully dissolved, the three-necked flask was moved to an ice-water bath. 183 g of o-hydroxybenzaldehyde was slowly added dropwise to the three-necked flask. After 2 hours of dropwise addition, the temperature was raised to 70°C and the reaction was continued for 48 hours. Then, 366 ml of a tetrahydrofuran solution of p-hydroxybenzaldehyde with a concentration of 0.5 g / ml was added dropwise to the three-necked flask. The reaction was continued for 48 hours, filtered and rotary evaporated to obtain an intermediate.
[0171] At room temperature, 315 g of dehydrated methyltriphenylphosphonium bromide and 500 ml of a dehydrated tetrahydrofuran solution of the intermediate with a concentration of 0.17 g / ml were added to a three-necked flask, stirred, and 170 g of freshly unsealed potassium tert-butoxide were slowly added. After reacting for 3 hours, 600 g of calcium bromide were added, and the reaction was stirred for 36 hours. An acetic acid aqueous solution was added to adjust the pH value to 7 to 8, and tetrahydrofuran in the system was removed by rotary evaporation. Ethyl acetate was added, and the liquid was separated. The oil phase was collected. After the ethyl acetate was removed by rotary evaporation, a mixed solution of cyclohexane and ethyl acetate was used as a mobile phase (cyclohexane: ethyl acetate = 500: 1-10: 1), and the product was separated and purified by a silica gel chromatography column to obtain a product labeled A5. The pH value was measured to be 8, and the specific structure is shown in formula (7).
[0172]
[0173] Homemade compound A6:
[0174] At room temperature, 201 g of dodecachlorocyclohexaphosphazene, 525 g of potassium carbonate and 400 ml of tetrahydrofuran were added to a three-necked flask. After sufficient dissolution, the three-necked flask was moved to an ice-water bath. 220 g of o-hydroxybenzaldehyde was slowly added dropwise to the three-necked flask. After 2 hours of dropwise addition, the temperature was raised to 70°C and the reaction was continued for 48 hours. Then, 440 ml of a tetrahydrofuran solution of p-hydroxybenzaldehyde with a concentration of 0.5 g / ml was added dropwise to the three-necked flask, the reaction was continued for 60 hours, and the intermediate was obtained by filtration and rotary evaporation.
[0175] At room temperature, 315 g of dehydrated methyltriphenylphosphonium bromide and 500 ml of a dehydrated tetrahydrofuran solution of an intermediate with a concentration of 0.17 g / ml were added to a three-necked flask, stirred, and 100 g of freshly unsealed potassium tert-butoxide was slowly added. After reacting for 3 hours, 600 g of calcium bromide was added, and the reaction was stirred for 24 hours. An acetic acid aqueous solution was added to adjust the pH value to 7 to 8, and tetrahydrofuran in the system was removed by rotary evaporation. Ethyl acetate was added, and the liquids were separated. The oil phase was collected. After the ethyl acetate was removed by rotary evaporation, a mixed solution of cyclohexane and ethyl acetate was used as a mobile phase (cyclohexane: ethyl acetate = 500: 1-10: 1), and the product was separated and purified by a silica gel chromatography column to obtain a product labeled A6. The pH value was measured to be 8, and the specific structure is shown in formula (8).
[0176]
[0177] Homemade compound A7:
[0178] At room temperature, 100 g of hexachlorocyclotriphosphazene, 270 g of potassium carbonate and 400 ml of tetrahydrofuran were added to a three-necked flask. After sufficient dissolution, the three-necked flask was moved to an ice-water bath. 110 g of o-hydroxybenzaldehyde was slowly added dropwise to the three-necked flask. After 2 hours of dropwise addition, the temperature was raised to 40°C and the reaction was continued for 72 hours. Then, 220 ml of a tetrahydrofuran solution of p-hydroxybenzaldehyde with a concentration of 0.5 g / ml was added dropwise to the three-necked flask, the reaction was continued for 48 hours, and the intermediate was obtained by filtering and rotary evaporation.
[0179] At room temperature, 315 g of dehydrated methyltriphenylphosphonium bromide and 500 ml of a dehydrated 0.17 g / ml tetrahydrofuran solution of the intermediate were added to a three-necked flask, stirred, and 100 g of freshly unsealed potassium tert-butoxide were slowly added. After reacting for 2 hours, 600 g of calcium bromide were added, and the reaction was stirred for 24 hours. An acetic acid aqueous solution was added to adjust the pH value to 3 to 4, and tetrahydrofuran in the system was removed by rotary evaporation. Ethyl acetate was added, and the liquids were separated. The oil phase was collected. After the ethyl acetate was removed by rotary evaporation, a mixed solution of cyclohexane and ethyl acetate was used as a mobile phase (cyclohexane: ethyl acetate = 500: 1-10: 1), and the product was separated and purified by a silica gel chromatography column to obtain a product labeled A7. The measured pH value was 4, and its structure was shown in the above formula (4).
[0180] Homemade compound A8:
[0181] At room temperature, 100 g of hexachlorocyclotriphosphazene, 270 g of potassium carbonate and 400 ml of tetrahydrofuran were added to a three-necked flask. After sufficient dissolution, the three-necked flask was moved to an ice-water bath. 110 g of o-hydroxybenzaldehyde was slowly added dropwise to the three-necked flask. After 2 hours of dropwise addition, the temperature was raised to 60°C and the reaction was continued for 56 hours. Then, 220 ml of a tetrahydrofuran solution of p-hydroxybenzaldehyde with a concentration of 0.5 g / ml was added dropwise to the three-necked flask. The reaction was continued for 48 hours, filtered and rotary evaporated to obtain an intermediate.
[0182] At room temperature, 315 g of dehydrated methyltriphenylphosphonium bromide and 500 ml of a dehydrated tetrahydrofuran solution of the intermediate with a concentration of 0.17 g / ml were added to a three-necked flask, and the mixture was stirred. 48 g of newly opened sodium methoxide was slowly added. After reacting for 2 hours, 600 g of calcium bromide was added. The mixture was stirred and reacted for 24 hours. An aqueous ammonium chloride solution was added to adjust the pH value to 11 to 12. The tetrahydrofuran in the system was removed by rotary evaporation. Ethyl acetate was added, the liquids were separated, and the oil phase was collected. After removing the ethyl acetate by rotary evaporation, a mixed solution of cyclohexane and ethyl acetate was used as a mobile phase (cyclohexane: ethyl acetate = 500: 1-10: 1). The product was separated and purified by a silica gel chromatography column to obtain a product labeled A8. The pH value was measured to be 11, and the structure thereof was shown in the aforementioned formula (4).
[0183] Homemade compound C1:
[0184] 31.2 g of NaH and 400 ml of tetrahydrofuran were added to a 1-liter three-necked flask, nitrogen was introduced, the temperature was raised to 50°C with stirring, 97.7 g of o-hydroxybenzaldehyde was dissolved in 200 ml of tetrahydrofuran, and the mixture was slowly added dropwise to the three-necked flask. After the addition was completed, the reaction was continued for 4 hours. Then, 34.7 g of hexachlorocyclotriphosphazene was dissolved in 200 ml of tetrahydrofuran, added to the three-necked flask, the temperature was raised to 65°C, the reaction was carried out for 48 hours, centrifuged, filtered and dried several times to obtain an intermediate product.
[0185] Add dry methyltriphenylphosphine bromide (150% excess) and calcium hydride (150% excess) to tetrahydrofuran, and then add the intermediate product. After the reaction is complete, add acetic acid and stir for 1 hour. Filter with suction to obtain compound C1. The pH value is 8. The structure of compound C1 is shown in formula (9).
[0186]
[0187] Homemade compound C2:
[0188] 31.2 g of NaH and 400 ml of tetrahydrofuran were added to a 1-liter three-necked flask, nitrogen was introduced, and the temperature was stirred and raised to 50°C. 48.85 g of o-hydroxybenzaldehyde and 37.6 g of phenol were dissolved in 200 ml of tetrahydrofuran and slowly added dropwise to the three-necked flask. After the addition was completed, the reaction was continued for 4 hours. 34.7 g of hexachlorocyclotriphosphazene was dissolved in 200 ml of tetrahydrofuran, added to the three-necked flask, and the temperature was raised to 65°C for reaction for 48 hours. The intermediate product was obtained by centrifugation, filtration and drying for multiple times.
[0189] Add dry methyltriphenylphosphine bromide (150% excess) and calcium hydride (140% excess) to tetrahydrofuran, add the intermediate product, add acetic acid after the reaction is complete, stir for 1 hour, filter, and obtain compound C2. The pH value is 8. The structure of compound C2 is shown in formula (10).
[0190]
[0191] Homemade compound C3:
[0192] In a 5L four-necked flask equipped with a thermometer, a stirrer, a condenser, and a dropping funnel, a tetrahydrofuran (800 ml) solution of hexachlorocyclotriphosphazene (243.4 g, 2.10 mol) was added under a nitrogen stream, and a pre-prepared tetrahydrofuran (2000 ml) solution of sodium 4-acetylphenolate (797.0 g, 5.04 mol) was added dropwise thereto at 10 to 20° C. for 3.5 hours, and then stirred under reflux for 15 hours. After the reaction mixture was cooled to room temperature, the solvent was distilled off under reduced pressure, diluted with toluene (2000 ml), 5% aqueous sodium hydroxide solution (500 ml) was added and transferred to a separating funnel. After the water layer was separated, the toluene layer was washed with 5% aqueous sodium hydroxide solution (500 ml), and then neutralized with dilute nitric acid and washed with water. The toluene layer was concentrated under reduced pressure to obtain 642.19 g of an intermediate product, which was a cyclic phosphazene compound containing acetylphenoxy.
[0193] A solution of a cyclic phosphazene compound containing acetylphenoxy group (315.26 g, 1.00 mol) in tetrahydrofuran (3000 ml) was added to a 5-liter autoclave under a nitrogen stream, and 10 wt% palladium-activated carbon (5.46 g) was added thereto. The autoclave was then pressurized with hydrogen and aged for 5 hours at room temperature. After confirming that the reaction was complete, Pd / C was filtered off, and tetrahydrofuran was removed by vacuum distillation to obtain 309.7 g of a product, which was compound C3, and the structure was shown in formula (11).
[0194]
[0195] Homemade compound C4:
[0196] Using hexachlorocyclotriphosphazene, 3-vinylphenol and phenol as main raw materials, a p-vinylbenzene cyclotriphosphazene compound, i.e., compound C4, is synthesized through a two-step nucleophilic substitution reaction by a stepwise addition method. The structure is shown in formula (12).
[0197]
[0198] Homemade compound C5:
[0199] Solvent, hexachlorocyclotriphosphazene, vinylphenol (a mixture of p-vinylphenol and m-vinylphenol in a ratio of 50:50), and an acid-binding agent are added to a reaction apparatus, stirred, and nitrogen is introduced for protection. The reaction apparatus is heated to 50-120° C. A catalyst is then added to the reaction apparatus. After reacting for 5-16 hours, the reaction apparatus is cooled to room temperature and filtered. The filtrate is subjected to pressure distillation and the solvent is evaporated to obtain a brown powder or a viscous product, namely compound C5, whose structure is shown in formula (13).
[0200]
[0201] Homemade compound C6:
[0202] With 4-allyloxy-4'-hydroxydiphenyl sulfone and sodium as the main raw materials, tetrahydrofuran was added at 25°C for substitution reaction to obtain 4-allyloxy-4'-oxysodium diphenyl sulfone, and then an appropriate amount of hexachlorocyclotriphosphazene and tetrahydrofuran were added. After removing NaCl at 60°C, compound C6 was obtained. The structure is shown in formula (14).
[0203]
[0204] Preparation of prepolymer 1:
[0205] 100 parts by weight of OPE-2st 2200, 10 parts by weight of A2 and 110 parts by weight of toluene were added to a Schlenk reaction bottle, and after uniform dissolution, 0.9 parts by weight of VR-110 (azo initiator) was added. Vacuum was evacuated under a liquid nitrogen environment, and nitrogen was passed through. The above steps were repeated three times to discharge oxygen in the system. The temperature was raised to 110° C., and after reacting for 3 hours, the self-made prepolymer 1 was obtained by cooling, filtering and purification, and the solid content of the self-made prepolymer 1 was 100%, and the conversion rate of the self-made prepolymer 1 was between 10% and 99%.
[0206] Preparation of prepolymer 2:
[0207] 50 parts by weight of OPE-2st 2200, 50 parts by weight of A2, 50 parts by weight of SA-9000 and 150 parts by weight of toluene were added to a Schlenk reaction bottle, and after uniform dissolution, 1.3 parts by weight of VR-110 were added. Vacuum was evacuated under a liquid nitrogen environment, and nitrogen was passed through. The above steps were repeated three times to discharge oxygen in the system. The temperature was raised to 100° C., and after reacting for 4 hours, the self-made prepolymer 2 was obtained after cooling, filtration and purification, and the solid content of the self-made prepolymer 2 was 100%, and the conversion rate of the self-made prepolymer 2 was between 10% and 99%.
[0208] The composition (unit: weight part) and characteristic test results of the resin compositions of the embodiments and comparative examples of the present invention are shown in the following table:
[0209] Table 1 Composition (unit: weight parts) of the resin composition of the embodiment and the test results of properties
[0210]
[0211]
[0212] Table 2 Composition (unit: weight parts) of the resin composition of the embodiment and the test results of properties
[0213]
[0214]
[0215] Table 3 Composition (unit: weight parts) of the resin composition of the embodiment and the test results of properties
[0216]
[0217]
[0218] Table 4 Composition (unit: weight parts) and characteristic test results of the resin composition of the comparative example
[0219]
[0220]
[0221] Table 5 Composition (unit: weight parts) and characteristic test results of the resin composition of the comparative example
[0222]
[0223]
[0224] The characteristic tests of the embodiments and comparative examples of the present application are performed by making the objects to be tested (test specimens, samples) in the following manner and then performing the tests according to specific test conditions.
[0225] 1) Precured sheet: The resin compositions in the examples or comparative examples are respectively selected and uniformly mixed to form a varnish, which is then injected into an impregnation tank. A glass fiber cloth (e.g., L-glass fiber fabric with a specification of 2116 or L-glass fiber fabric with a specification of 1080, both purchased from Asahi Co., Ltd.) is then immersed in the impregnation tank to adhere the resin composition to the glass fiber cloth, and the mixture is heated at 150° C. to 170° C. to a semi-cured state (B-Stage), thereby obtaining a precured sheet.
[0226] 2) Copper foil substrate (8-ply, 8 prepregs pressed together): 2 ultra-low surface roughness (HVLP) copper foils with a thickness of 18 microns and 8 2116 L-glass fiber cloths were prepared to impregnate the prepregs prepared by the samples to be tested (each group of examples or comparative examples). The resin content of each prepreg was about 53%. One HVLP copper foil, eight prepregs and one HVLP copper foil were stacked in the order of one HVLP copper foil, eight prepregs and one HVLP copper foil, and pressed together for 2 hours under vacuum conditions, a pressure of 420 psi, and 200° C. to form a copper foil substrate. Among them, the 8 stacked prepregs were cured to form an insulating layer between the two copper foils, and the resin content of the insulating layer was about 53%.
[0227] 3) Copper-free substrate (8-ply, formed by pressing together 8 prepregs): The above copper foil substrate (8-ply) is etched to remove 2 copper foils to obtain a copper-free substrate (8-ply), which is formed by pressing together 8 prepregs. The resin content of the copper-free substrate is about 53%.
[0228] 4) Copper-free substrate (2-ply, formed by laminating two prepregs): prepare two ultra-low surface roughness (HVLP) copper foils with a thickness of 18 microns and two 1080 L-glass fiber cloths to impregnate the prepregs made from each sample to be tested (each group of embodiments or comparative examples), and stack them in the order of copper foil, two prepregs, and copper foil, and press them for 2 hours under vacuum conditions, a pressure of 420 psi, and 200° C. to form a copper-containing substrate (2-ply, formed by laminating two prepregs). Then, the copper-containing substrate (2-ply) is etched to remove the copper foil on both sides to obtain a copper-free substrate (2-ply), which is formed by laminating two prepregs, and the resin content of the copper-free substrate (2-ply) is about 70%.
[0229] For the aforementioned samples to be tested, the test methods and their characteristic analysis items are as follows:
[0230] 1. Filling
[0231] A 2.5 mil thick copper-containing substrate (e.g., product EM-827, available from Taiwan Optoelectronic Materials Co., Ltd.) was processed into a browned circuit board through a known browning process as the inner layer to evaluate the ability of the prepreg to flow and fill the empty areas between the circuits during lamination. The varnish of the resin composition of each group of embodiments or comparative examples was impregnated with 1017 L-glass fiber cloth, and baked at 140°C for 4 minutes to obtain a prepreg, and the resin content of the prepreg was about 79%. The 2.5 mil thick browned circuit board was laminated on both sides of the aforementioned prepreg (a prepreg obtained by impregnating 1017 L-glass fiber cloth with each sample to be tested (each group of embodiments or comparative examples)), and an ultra-low surface roughness copper foil (thickness of 18 microns) was laminated on the outer layer. In a vacuum press, it was pressed for 2 hours at a pressure of 450psi and a temperature of 210°C to form an inner layer circuit substrate with a copper surface, and the outer copper foil was removed by etching to obtain an inner layer circuit substrate without copper on the surface. Repeat the above steps to make 15 inner circuit substrates without copper. Use an optical microscope to observe whether there is a shadow on the copper-free surface of the inner circuit substrate without copper. If there is a shadow on the surface, it means that the filling is poor, which will cause the subsequent circuit board to be scrapped. If at least one of the 15 inner circuit substrate samples without copper has a shadow on the surface (such as Figure 1 If there is no shadow on the surface of the 15 inner circuit substrate samples without copper (such as Figure 2As shown in the figure, it is marked as "pass", which means excellent filling performance.
[0232] 2. Interface adhesion
[0233] Select the aforementioned copper-free substrate (8-ply), cut a suitable size of glue-filled slices from the middle of the board, and use a Hitachi Regulus 8100 scanning electron microscope to observe whether there is a gap between the resin and the warp or weft glass fibers at a magnification of 10,000 times. If there is a gap, Figure 3 As shown, the mark "NG" means that the interface adhesion between the resin matrix and the glass fiber is poor and unqualified. Figure 4 As shown, it is marked as "pass", which means that the interface adhesion between the resin matrix and the glass fiber is excellent and qualified.
[0234] 3. Interconnect stress test (IST)
[0235] Interconnect stress test, also known as DC induction thermal cycle test, is a rapid method for thermal stress testing of finished PCB boards. It is used to evaluate the reliability of the interconnect structure (via) of the finished PCB.
[0236] According to the following structural description, the resin composition in the embodiment or comparative example is made into a 26-layer PCB board sample, dried, and then the PCB board sample is tested for the resistance value change rate after 1000 cycles of room temperature-150°C-room temperature (heating for 3 minutes, cooling for 2 minutes, 5 minutes as one cycle) using the interconnect stress test equipment model IST-HC produced by PWB Company, with reference to the method of IPC-TM-650 2.6.26. If the resistance value change rate is greater than or equal to 10%, it means unqualified, and it is marked as "NG", otherwise, if the resistance value change rate is less than 10%, it means qualified, and it is marked as "pass".
[0237] The structure design of the 26-layer PCB sample for interconnect stress testing is as follows:
[0238] L1 1 Hoz thick ultra-low surface roughness (HVLP) copper foil (made into circuit)
[0239] 2 sheets of 106 L-glass fiber cloth with 75% resin content prepreg
[0240] L2 1 Hoz thick ultra-low surface roughness (HVLP) copper foil (made into circuit)
[0241] 1 sheet of 3 mil 1086 L-glass cloth core board
[0242] L3 1 Hoz thick ultra-low surface roughness (HVLP) copper foil (made into circuit)
[0243] 2 sheets of 106 L-glass fiber cloth with 75% resin content prepreg
[0244] L4 1 Hoz thick ultra-low surface roughness (HVLP) copper foil (made into circuit)
[0245] 1 sheet of 3 mil 1086 L-glass cloth core board
[0246] L5 1 Hoz thick ultra-low surface roughness (HVLP) copper foil (made into circuit)
[0247] 2 sheets of 106 L-glass fiber cloth with 75% resin content prepreg
[0248] L6 1 loz thick ultra-low surface roughness (HVLP) copper foil (made into circuit)
[0249] 2 sheets of 1037 L-glass fiber cloth with a total thickness of 3.5 mils core board
[0250] L7 1 loz thick ultra-low surface roughness (HVLP) copper foil (made into circuit)
[0251] 2 sheets of 106 L-glass fiber cloth with 75% resin content prepreg
[0252] L8 1 loz thick ultra-low surface roughness (HVLP) copper foil (made into circuit)
[0253] 2 sheets of 1037 L-glass fiber cloth with a total thickness of 3.5 mils core board
[0254] L9 1 loz thick ultra-low surface roughness (HVLP) copper foil (made into circuit)
[0255] 2 sheets of 106 L-glass fiber cloth with 75% resin content prepreg
[0256] L10 1 loz thick ultra-low surface roughness (HVLP) copper foil (made into circuit)
[0257] 2 sheets of 4 mil total thickness 106 L-glass fiber cloth core board (enclosed area)
[0258] L11 1 sheet of 2oz thick ultra-low surface roughness (HVLP) copper foil
[0259] 2 sheets of 1080 L-glass cloth with 71% resin content prepreg
[0260] L12 1 sheet of 1oz thick ultra-low surface roughness (HVLP) copper foil (made into circuit)
[0261] 2 sheets of 4 mil total thickness 106 L-glass fiber cloth core board
[0262] L13 1 sheet of 2oz thick ultra-low surface roughness (HVLP) copper foil (made into circuit)
[0263] 3 sheets of 1080 L-glass fiber cloth with 71% resin content prepreg
[0264] L14 1 sheet of 2oz thick ultra-low surface roughness (HVLP) copper foil (made into circuit)
[0265] 2 sheets of 4 mil total thickness 106 L-glass fiber cloth core board
[0266] L151 loz thick ultra-low surface roughness (HVLP) copper foil (made into circuits)
[0267] 2 sheets of 1080 L-glass cloth with 71% resin content prepreg
[0268] L16 1 sheet of 2oz thick ultra-low surface roughness (HVLP) copper foil
[0269] 2 sheets of 4 mil total thickness 106 L-glass fiber cloth core board (enclosed area)
[0270] L17 1 sheet of 1oz thick ultra-low surface roughness (HVLP) copper foil (made into circuit)
[0271] 2 sheets of 106 L-glass fiber cloth with 75% resin content prepreg
[0272] L18 1 sheet of 1oz thick ultra-low surface roughness (HVLP) copper foil (made into circuit)
[0273] 2 sheets of 1037 L-glass fiber cloth with a total thickness of 3.5 mils core board
[0274] L19 1 sheet of 1oz thick ultra-low surface roughness (HVLP) copper foil (made into circuit)
[0275] 2 sheets of 106 L-glass fiber cloth with 75% resin content prepreg
[0276] L20 1 loz thick ultra-low surface roughness (HVLP) copper foil (made into circuit)
[0277] 2 sheets of 1037 L-glass fiber cloth with a total thickness of 3.5 mils core board
[0278] L21 1 loz thick ultra-low surface roughness (HVLP) copper foil (made into circuit)
[0279] 2 sheets of 106 L-glass fiber cloth with 75% resin content prepreg
[0280] L22 1 Hoz thick ultra-low surface roughness (HVLP) copper foil (made into circuit)
[0281] 1 sheet of 3 mil 1086 L-glass cloth core board
[0282] L23 1 Hoz thick ultra-low surface roughness (HVLP) copper foil (made into circuit)
[0283] 2 sheets of 106 L-glass fiber cloth with 75% resin content prepreg
[0284] L24 1 Hoz thick ultra-low surface roughness (HVLP) copper foil (made into circuit)
[0285] 1 sheet of 3 mil 1086 L-glass cloth core board
[0286] L25 1 Hoz thick ultra-low surface roughness (HVLP) copper foil (made into circuit)
[0287] 2 sheets of 106 L-glass fiber cloth with 75% resin content prepreg
[0288] L26 1 Hoz thick ultra-low surface roughness (HVLP) copper foil (made into circuit)
[0289] Among them, 1oz copper foil corresponds to a thickness of 35 microns, Hoz copper foil corresponds to a copper foil thickness of 18 microns, and so on.
[0290] 4. Dielectric loss aging rate (Df aging rate)
[0291] The aforementioned copper-free substrate (2-ply) was measured for dielectric loss value Df1 of each sample at room temperature (about 25°C) and at a frequency of 10 GHz using a microwave dielectrometer (purchased from AET, Japan) with reference to the method of JIS C2565. After the test, the sample was placed in a constant temperature and humidity chamber at a temperature of 85°C and a relative humidity of 85% for 500 hours to absorb moisture, and the dielectric loss value Df2 was tested again. Calculated using the formula: Df aging rate = ((Df2 after aging - Df1 before aging) / Df1 before aging) × 100%.
[0292] 5. Bonding strength (B / S)
[0293] The copper foil substrate (composed of eight prepregs pressed together) was cut into a rectangle with a width of 12.7 mm and a length greater than 60 mm, and was measured using a universal tensile strength tester and with reference to the method of IPC-TM-650 2.4.8. The surface copper foil does not need to be etched during the process, and the test position is the bonding surface between the second layer of prepreg and the third layer of prepreg. The force (lb / in) required to separate the two layers of the cured insulating substrate was tested at room temperature (about 25°C). For copper foil substrates with a Df value of less than 0.005 measured at a frequency of 10 GHz for dielectric loss, a significant difference is considered to exist if the difference in interlayer bonding force is greater than 0.1 lb / in.
[0294] 6. Temperature coefficient of dielectric constant (TcDk)
[0295] The aforementioned copper-free substrate (2-ply) was cut into square samples of 8 cm×8 cm, and the SPDR resonant cavity analyzer (split post dielectric resonant cavity, purchased from Waveray) was used to measure the change of the dielectric constant Dk of the sample at a frequency of 10 GHz and a relative humidity of 65%, and the temperature range of the sample was between 25°C and 150°C according to the method of IPC-TM-6502.5.5.13. The smaller the value of the dielectric constant temperature coefficient TcDk, the smaller the change value of the dielectric constant Dk when the temperature rises, which means that the dielectric constant of the insulation layer of the copper-free substrate is more stable, and the signal transmission of the subsequently manufactured printed circuit board in a high temperature environment is also more stable.
[0296] 7. Temperature coefficient of dielectric loss factor (TcDf)
[0297] The aforementioned copper-free substrate (2-ply) was cut into 8cm×8cm square samples, and the SPDR resonant cavity analyzer (split post dielectric resonant cavity, purchased from Waveray) was used to measure the change of the dielectric loss Df of the sample at a frequency of 10GHz and a relative humidity of 65%, and the temperature range of the sample was between 25°C and 150°C according to the method of IPC-TM-6502.5.5.13. The smaller the value of the dielectric loss temperature coefficient TcDf, the smaller the change value of the dielectric loss Df when the temperature rises, which means that the dielectric loss of the insulation layer of the copper-free substrate is more stable, and the signal integrity of the subsequently manufactured printed circuit board in a high temperature environment is better.
[0298] By referring to the characteristic test results in Tables 1 to 5, the following phenomena can be clearly observed:
[0299] By comparing Examples E12 to E13 with other Examples, it can be determined that the resin composition of the present invention, whether it is a technical solution comprising a polyphenylene ether resin containing unsaturated carbon-carbon double bonds and a compound of formula (1) (whose pH value is 5 to 10), or a technical solution comprising a prepolymer obtained by prepolymerizing a polyphenylene ether resin containing unsaturated carbon-carbon double bonds and a compound of formula (1) (whose pH value is 5 to 10), can also be improved in one or more aspects such as filling property, interface adhesion, interconnect stress test, dielectric loss aging rate, interlayer bonding strength, dielectric constant temperature coefficient TcDk, and dielectric loss temperature coefficient TcDf.
[0300] By comparing Examples E1, E2, and E4 with Comparative Examples C1 and C2, it can be found that if the amount of the compound of formula (1) is not within the range of 10 to 50 parts by weight, the properties of the sample in terms of filling properties, interface adhesion, interconnect stress testing, interlayer bonding strength, etc. cannot be significantly improved.
[0301] By comparing the various embodiments with comparative examples C3 and C4, it can be found that if the pH value of the compound of formula (1) is less than 5 or greater than 10, the sample cannot be significantly improved in one or more aspects such as filling property, interface adhesion, interconnect stress test, dielectric loss aging rate, interlayer bonding strength, dielectric constant temperature coefficient TcDk, and dielectric loss temperature coefficient TcDf.
[0302] By comparing the various embodiments with comparative examples C5 to C12, it can be found that if the compound of formula (1) (whose pH value is 5 to 10) is not used but only other compounds with a structure different from that of the compound of formula (1) are used, the properties of the sample cannot be significantly improved at least in terms of interlayer bonding strength, dielectric constant temperature coefficient TcDk, dielectric loss temperature coefficient TcDf, etc.
[0303] Compared with the embodiments E12-E13 using prepolymers and other embodiments using a resin composition of a polyphenylene ether resin containing unsaturated carbon-carbon double bonds and a compound of formula (1) (whose pH value is 5 to 10), E12-E13 have lower dielectric loss aging rate and higher interlayer bonding strength.
[0304] By comparing Examples EI-E8 and E9-E15 of the present invention, it can be determined that the products prepared by further adding phosphate flame retardants to the resin composition can further significantly improve the characteristics of the dielectric loss aging rate, dielectric loss temperature coefficient TcDf, etc.
[0305] The above implementation modes and examples are essentially only auxiliary explanations and are not intended to limit the embodiments of the present application or the application or use of these embodiments. In the present application, a term similar to "example" means "as an example, paradigm or illustration". Any exemplary embodiment herein is not necessarily interpreted as being preferred or more advantageous relative to other embodiments, unless otherwise specified.
[0306] In addition, although at least one exemplary embodiment or comparative example has been proposed in the aforementioned embodiment, it should be understood that a large number of variations may still exist in the present application. It should also be understood that the embodiments herein are not intended to limit the scope, use or configuration of the requested technical solution in any way. On the contrary, the aforementioned embodiment can provide a simple guide for those skilled in the art to implement one or more of the aforementioned embodiments and their equivalents. In addition, the claims include known equivalents and all foreseeable equivalents when the present patent application is filed.
Claims
1. A resin composition, characterized in that Contains the following ingredients or their prepolymers: (A) 100 parts by weight of a polyphenylene ether resin containing unsaturated carbon-carbon double bonds; and (B) 10 to 50 parts by weight of a compound of formula (1), wherein the pH value of the compound of formula (1) is 5 to 10; In formula (1), n is an integer from 3 to 6, X and Y are each independently o-vinylphenoxy or p-vinylphenoxy, and X and Y are not both o-vinylphenoxy and p-vinylphenoxy; The prepolymer is obtained by prepolymerization of a mixture, and the mixture includes the component (A) and the component (B).
2. The resin composition according to claim 1, characterized in that The prepolymer is formed by prepolymerization of the component (A) and the component (B), and the conversion rate of the prepolymerization is between 10% and 99%.
3. The resin composition according to claim 1, characterized in that The polyphenylene ether resin containing unsaturated carbon-carbon double bonds includes any one of vinylbenzyl polyphenylene ether resin, (meth)acryl polyphenylene ether resin, vinyl polyphenylene ether resin or a combination thereof.
4. The resin composition according to claim 1, characterized in that The resin composition further comprises polyolefin, and the amount of the polyolefin is 5 parts by weight to 25 parts by weight relative to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds.
5. The resin composition according to claim 1, characterized in that The resin composition further comprises any one or a combination of bis(vinylphenyl)ethane, divinylbenzene, divinylnaphthalene, divinylbiphenyl, tert-butylstyrene, triallyl isocyanurate, triallyl cyanurate, vinylbenzocyclobutene, di(vinylbenzyl)ether, trivinylcyclohexane, diallyl isophthalate, diallyl bisphenol A, acrylate, butadiene, decadiene, octadiene, vinylcarbazole, and styrene.
6. The resin composition according to claim 1, characterized in that The resin composition further comprises any one of epoxy resin, polyester resin, phenol resin, amine curing agent, polyamide, polyimide, styrene maleic anhydride, cyanate ester or a combination thereof.
7. The resin composition according to claim 1, characterized in that The resin composition further comprises any one of an inorganic filler, a flame retardant, a hardening accelerator, an inhibitor, a solvent, a silane coupling agent, a dye, and a toughening agent, or a combination thereof.
8. The resin composition according to claim 1, characterized in that The resin composition further comprises a phosphate flame retardant, and the mass ratio of the compound of formula (1) to the phosphate flame retardant is between 1.5:1.0 and 25.0:1.
0.
9. A product made from the resin composition according to any one of claims 1 to 8, characterized in that: The product includes a prepreg, a resin film, a laminate or a printed circuit board.
10. The product according to claim 9, characterized in that The product has one or more of the following characteristics: The resistance change rate after 1000 cycles measured by the interconnect stress test according to IPC-TM-6502.6.26 is less than 10%; The interlayer bonding strength measured according to IPC-TM-6502.4.8 is greater than or equal to 3.5 lb / in; The dielectric constant temperature coefficient measured according to IPC-TM-6502.5.5.13 is less than or equal to 73ppm / ℃; The dielectric loss temperature coefficient measured according to IPC-TM-6502.5.5.13 is less than or equal to 6300ppm / C; After the product is left to stand for 500 hours in an environment with a temperature of 85° C. and a relative humidity of 85%, the dielectric loss aging rate calculated by measuring the dielectric loss at a frequency of 10 GHz according to the method of JIS C2565 is less than or equal to 57%.
Citation Information
Cited By
Resin composition and product of the same
TWI939019B