Polyurethane composite material, polyurethane foam material and preparation method and application thereof

By utilizing the good compatibility of soft and hard polyurethanes in polyurethane composites, a polyurethane foamed material with bimodal cell structure was prepared, which solved the difficulty in preparing bimodal cell structures in the prior art by polymer blending method. and realizes the efficient heat insulation and sound absorption effect of the material and complete recycling.

CN119060526AActive Publication Date: 2024-12-03EAST CHINA UNIV OF SCI & TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411224782.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-12-03
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

The prior art is difficult to effectively prepare polymer foamed materials with bimodal cell structures, and heterogeneous polymers have poor compatibility and are difficult to recycle.

Method used

Using polyurethane composite materials, including soft polyurethane and rigid polyurethane, the bimodal cell structure is prepared through good compatibility, and the pressure relief foaming is performed by using the CO2 environment to control the melt blending temperature and proportion to adjust the cell size. .

Benefits of technology

The bimodal cell structure of polyurethane foaming material is realized, which improves the heat insulation and sound absorption effect of the material, and due to its good compatibility, the material can be completely recycled.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060526A_ABST
    Figure CN119060526A_ABST
Patent Text Reader

Abstract

The invention provides a polyurethane composite material, a polyurethane foaming material and a preparation method and application thereof, and belongs to the technical field of polymer foaming materials. The invention provides a polyurethane composite material. The polyurethane composite material comprises a polyurethane matrix and a polyurethane compound dispersed in the matrix, the polyurethane compound is prepared from soft polyurethane and hard polyurethane; and the polyurethane matrix is made of soft polyurethane. The soft polyurethane and the hard polyurethane in the matrix are polyurethane, so that the soft polyurethane and the hard polyurethane have good compatibility, the hard polyurethane and the soft polyurethane are firstly prepared into a compound, and then the compound is dispersed in the soft polyurethane matrix, so that the compatibility of the hard polyurethane and the soft polyurethane matrix is further improved; due to the good compatibility, the prepared foaming material has a double-peak cellular structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer foam materials, and in particular to a polyurethane composite material, a polyurethane foam material, and a preparation method and application thereof. Background Art

[0002] Polymer foam material is a polymer material with a polymer matrix and a large number of pore structures inside. Among them, thermoplastic polyurethane (TPU) is a block copolymer composed of soft and hard segments, with excellent elasticity, wear resistance, easy processing and structural versatility. Its foam material has light weight, high resilience, excellent mechanical strength and flexibility, and is widely used in high-end shoe materials, electromagnetic shielding materials, polishing pads and flexible sensors. Compared with TPU foam materials with uniform pore structure, TPU foam materials with bimodal pore structure have better heat insulation and sound absorption effects. Small pores provide good mechanical properties, and large pores can reduce the apparent density of the material and improve the resilience of the material. In recent years, it has received extensive attention and research from academia and industry.

[0003] At present, the method for preparing bimodal cellular polymer foam materials includes polymer blending. The polymer blending method is to melt and blend two polymers with different affinities with CO2. During the foaming process, the solubility of CO2 in the two phases is different, thereby preparing a polymer foam material with a bimodal cellular structure, such as TPU / polydimethylsiloxane (PDMS) blends, but the heterogeneous polymers have poor compatibility and are difficult to recycle. Summary of the invention

[0004] The invention provides a polyurethane composite material, a polyurethane foaming material and a preparation method and application thereof. The raw materials in the polyurethane composite material of the invention have good compatibility.

[0005] The present invention provides a polyurethane composite material, comprising a polyurethane matrix and a polyurethane compound dispersed in the matrix; the polyurethane compound comprises soft polyurethane and hard polyurethane;

[0006] The polyurethane matrix is ​​soft polyurethane.

[0007] Preferably, the mass ratio of soft polyurethane to hard polyurethane in the polyurethane composite is 2 to 99:1.

[0008] Preferably, the polyurethane composite has a shape including fiber and / or spherical.

[0009] Preferably, when the polyurethane composite is in a fibrous shape, the diameter of the polyurethane composite is 100 to 150 μm.

[0010] Preferably, the mass ratio of the polyurethane matrix to the polyurethane composite is 4 to 99:1.

[0011] Preferably, the melting temperature of the rigid polyurethane is 20-40° C. higher than the melting temperature of the soft polyurethane.

[0012] The present invention also provides a method for preparing a polyurethane foam material, comprising the following steps:

[0013] The polyurethane composite material described in the above technical solution is saturated in a CO2 environment and then pressure-released for foaming to obtain the polyurethane foam material.

[0014] Preferably, the saturation temperature is 10-40° C. lower than the melting temperature of the soft polyurethane in the polyurethane composite material.

[0015] The present invention also provides a polyurethane foam material prepared by the preparation method described in the above technical scheme, which has a bimodal pore structure; the average pore diameter of the small pores in the bimodal pore structure is 0.4-2.5 μm, and the average pore diameter of the large pores is 20-40 μm.

[0016] The present invention also provides the use of the polyurethane foam material described in the above technical solution in the fields of shoe materials, electromagnetic shielding materials, polishing pads or flexible sensors.

[0017] The present invention provides a polyurethane composite material, comprising a polyurethane matrix and a polyurethane compound dispersed in the matrix; the polyurethane compound comprises soft polyurethane and hard polyurethane;

[0018] The polyurethane matrix is ​​soft polyurethane.

[0019] The soft polyurethane in the matrix of the present invention and the hard polyurethane in the polyurethane composite are both polyurethanes, so the two have good compatibility. In addition, the hard polyurethane and the soft polyurethane are first prepared into a composite and then dispersed in the soft polyurethane matrix, which further improves the compatibility of the hard polyurethane and the soft polyurethane matrix. The good compatibility enables the prepared foam material to have a bimodal pore structure.

[0020] Furthermore, the present invention can controllably adjust the size of the pores by changing the melt blending temperature, the ratio of the hard polyurethane to the soft polyurethane in the polyurethane composite, and the saturation temperature. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a SEM image of the cross section of the TPU foam material prepared in Example 3;

[0022] Figure 2 The SEM image of the cross section of the TPU foam material prepared in Comparative Example 1;

[0023] Figure 3 This is the SEM image of the cross section of the TPU foam material prepared in Comparative Example 2. DETAILED DESCRIPTION

[0024] The present invention provides a polyurethane composite material, comprising a polyurethane matrix and a polyurethane compound dispersed in the matrix; the polyurethane compound comprises soft polyurethane and hard polyurethane;

[0025] The polyurethane matrix is ​​soft polyurethane.

[0026] In the present invention, the polyurethane composite material comprises a polyurethane matrix; the polyurethane matrix is ​​a soft polyurethane;

[0027] In the present invention, the polyurethane composite material comprises a polyurethane compound dispersed in a matrix.

[0028] In the present invention, the mass ratio of the polyurethane matrix and the polyurethane composite is preferably 4 to 99:1, more preferably 17 to 60:1, and further preferably 30 to 50:1; the polyurethane composite comprises soft polyurethane and hard polyurethane; the mass ratio of soft polyurethane to hard polyurethane in the polyurethane composite is preferably 2 to 99:1, more preferably 17 to 60:1, and further preferably 40 to 50:1.

[0029] In the present invention, the melting temperature of the rigid polyurethane is preferably 20 to 40°C higher than the melting temperature of the soft polyurethane, more preferably 15 to 30°C; the number average molecular weights of the rigid polyurethane and the soft polyurethane are preferably independently 100,000 to 400,000, more preferably 150,000 to 300,000, and further preferably 200,000 to 250,000.

[0030] In the present invention, the rigid polyurethane and the soft polyurethane are preferably prepared from the same type of diisocyanate, chain extender and polyester / polyether polyol. The rigid polyurethane and the soft polyurethane differ only in the hard segment content.

[0031] In the present invention, the shape of the polyurethane composite preferably includes fiber and / or spherical; when the shape of the polyurethane composite is fiber, the diameter of the polyurethane composite is preferably 100 to 150 μm, more preferably 120 to 130 μm;

[0032] The method for preparing the fibrous polyurethane composite preferably comprises: mixing soft polyurethane and hard polyurethane and then performing melt spinning.

[0033] In the present invention, before the mixing, it is preferred that the soft polyurethane and the hard polyurethane are dried separately.

[0034] The spinning temperature during the melt spinning is preferably 30 to 50°C higher than the melting temperature of the rigid polyurethane, more preferably 40 to 45°C; the drawing temperature is preferably 50 to 80°C lower than the melting temperature of the soft polyurethane, more preferably 60 to 70°C; the drawing multiple is preferably 3.0 to 8.0 times, more preferably 4 to 5 times.

[0035] In the present invention, the method for preparing the polyurethane composite material preferably comprises the following steps: melt-blending the polyurethane matrix and the polyurethane composite.

[0036] In the present invention, the temperature of the melt blending is preferably 20 to 40°C higher than the melting temperature of the soft polyurethane; the time is preferably 3 to 10 minutes, more preferably 5 to 8 minutes; the melt blending is preferably carried out in a torque rheometer, and the screw speed of the torque rheometer is preferably 40 to 70 rpm, more preferably 50 to 60. The screw speed is 40 to 70 rpm.

[0037] The present invention also provides a method for preparing a polyurethane foam material, comprising the following steps:

[0038] The polyurethane composite material described in the above technical solution is saturated in a CO2 environment and then pressure-released for foaming to obtain the polyurethane foam material.

[0039] In the present invention, the saturation temperature is preferably 10 to 40°C lower than the melting temperature of the soft polyurethane, and more preferably 20 to 30°C; the pressure is preferably 10 to 20 MPa, and more preferably 12 to 16 MPa; the time is preferably 0.5 to 1.5 h, and more preferably 0.8 to 1.2 h; the pressure relief rate of the pressure relief foaming is preferably 100 to 300 MPa / s, and more preferably 120 to 250 MPa / s, and more preferably 150 to 200 MPa / s.

[0040] The present invention also provides a polyurethane foam material prepared by the above technical solution, which has a bimodal pore structure; the average pore diameter of small pores in the bimodal pore structure is 0.4-2.5 μm, and the average pore diameter of large pores is 20-40 μm.

[0041] The hard polyurethane in the polyurethane composite material forms small cells; the soft polyurethane matrix forms large cells.

[0042] In the present invention, the hard polyurethane and the soft polyurethane are preferably thermoplastic materials. When they are thermoplastic materials, the polyurethane foam material can be completely recycled.

[0043] In the present invention, the average pore size of the large cells is preferably more than 10 times the pore size of the small cells; the foaming ratio of the polyurethane foam material is preferably 3 to 8 times, more preferably 4 to 6 times.

[0044] The present invention also provides the application of the polyurethane foam material described in the above technical solution in the fields of shoe materials, electromagnetic shielding materials, polishing pads and flexible sensors.

[0045] The polyurethane composite material, polyurethane foam material, preparation method and application thereof provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0046] Hard TPU granules (TPU1160D) and soft TPU granules (TPU1180A), BASF Shanghai Co., Ltd.

[0047] Example 1

[0048] The hard TPU particles and soft TPU particles were vacuum dried at 100°C and 70°C for 12 hours respectively to remove moisture. The two dried particles (the mass ratio of hard TPU particles to soft TPU particles is 1:99) were mixed and melt-spun to prepare hard TPU continuous fiber masterbatch. During the spinning process, the screw temperature was 210-225°C, the traction temperature was 75°C, the traction multiple was 8 times, and the diameter of the prepared fiber was 100 μm; the hard TPU continuous fiber with a mass ratio of 5:95 and the soft TPU particles were melt-blended by a torque rheometer to prepare a TPU composite material, the processing temperature was 175°C, the screw speed was 50 rpm, and the processing time was 4 min; saturated at 130°C and 15MPa CO2 for 1.5 hours, and rapidly decompressed at a speed of 300MPa / s to prepare a TPU foaming material.

[0049] Example 2

[0050] The hard TPU particles and soft TPU particles were vacuum dried at 100°C and 70°C for 12 hours respectively to remove moisture, and the two dried particles (the mass ratio of hard TPU particles to soft TPU particles was 3:97) were melt-spun to prepare hard TPU continuous fiber masterbatch. During the spinning process, the screw temperature was 210-225°C, the traction temperature was 75°C, the traction multiple was 8 times, and the diameter of the prepared fiber was 100 μm; the hard TPU continuous fiber with a mass ratio of 5:95 and the soft TPU particles were melt-blended by a torque rheometer to prepare a TPU composite material, the processing temperature was 175°C, the screw speed was 50 rpm, and the processing time was 4 min; saturated at 130°C and 15MPa CO2 for 1.5 hours, and rapidly decompressed at a rate of 300MPa / s to prepare a TPU foaming material.

[0051] Example 3

[0052] The hard TPU particles and soft TPU particles were vacuum dried at 100°C and 70°C for 12 hours respectively to remove moisture, and the two dried particles (the mass ratio of hard TPU particles to soft TPU particles was 5:95) were melt-spun to prepare hard TPU continuous fiber masterbatch. During the spinning process, the screw temperature was 210-225°C, the traction temperature was 75°C, the traction multiple was 8 times, and the diameter of the prepared fiber was 100 μm; the hard TPU continuous fiber with a mass ratio of 5:95 and the soft TPU particles were melt-blended by a torque rheometer to prepare a TPU composite material, the processing temperature was 175°C, the screw speed was 50 rpm, and the processing time was 4 min; saturated at 130°C and 15MPa CO2 for 1.5 hours, and rapidly decompressed at a speed of 300MPa / s to prepare a TPU foaming material.

[0053] Example 4

[0054] The hard TPU particles and soft TPU particles were vacuum dried at 100°C and 70°C for 12 hours respectively to remove moisture, and the two dried particles (the mass ratio of hard TPU particles to soft TPU particles was 7:93) were melt-spun to prepare hard TPU continuous fiber masterbatch. During the spinning process, the screw temperature was 210-225°C, the traction temperature was 75°C, the traction multiple was 8 times, and the diameter of the prepared fiber was 100 μm; the hard TPU continuous fiber with a mass ratio of 5:95 and the soft TPU particles were melt-blended by a torque rheometer to obtain a TPU composite material, the processing temperature was 175°C, the screw speed was 50 rpm, and the processing time was 4 min; saturated at 130°C and 15MPa CO2 for 1.5 hours, and the TPU foaming material was prepared by rapid pressure relief at a speed of 300MPa / s.

[0055] Comparative Example 1

[0056] The soft TPU particles were vacuum dried at 70°C to remove moisture, and the TPU samples were melted by a torque rheometer. The processing temperature was 175°C, the screw speed was 50 rpm, and the processing time was 4 min. The particles were saturated at 130°C and 15 MPa CO2 for 1.5 h, and the TPU foam material was prepared by rapid pressure release at a speed of 300 MPa / s.

[0057] Comparative Example 2

[0058] The hard TPU particles were vacuum dried at 100°C for 12 hours to remove moisture, and melt-spun to prepare hard TPU continuous fiber masterbatch. During the spinning process, the screw temperature was 210-225°C, the traction temperature was 75°C, the traction multiple was 8 times, and the diameter of the prepared fiber was 100 μm; the hard TPU continuous fiber and soft TPU particles with a mass ratio of 5:95 were melt-blended with a torque rheometer to prepare a TPU composite material, the processing temperature was 175°C, the screw speed was 50 rpm, and the processing time was 4 min; saturated at 130°C and 15 MPa CO2 for 1.5 hours, and rapidly decompressed at a speed of 300 MPa / s to prepare a TPU foaming material.

[0059] The cross section of the TPU foam material prepared in Example 3 was subjected to SEM analysis, and the results were as follows: Figure 1 shown.

[0060] The cross section of the TPU foam material prepared in Comparative Example 1 was subjected to SEM analysis, and the results were as follows: Figure 2 shown.

[0061] The cross section of the TPU foam material prepared in Comparative Example 2 was subjected to SEM analysis, and the results were as follows: Figure 3 shown.

[0062] Depend on Figures 1 to 3 It can be seen that the bimodal pore structure can only be prepared by first forming a hard TPU continuous fiber masterbatch from hard TPU and soft TPU, and then compounding it with soft TPU to prepare a TPU composite material.

[0063] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A polyurethane composite material, characterized in that: It comprises a polyurethane matrix and a polyurethane compound dispersed in the matrix; the polyurethane compound comprises soft polyurethane and hard polyurethane; The polyurethane matrix is ​​soft polyurethane.

2. The polyurethane composite material according to claim 1, characterized in that: The mass ratio of soft polyurethane to hard polyurethane in the polyurethane composite is 2 to 99:

1.

3. The polyurethane composite material according to claim 1, characterized in that: The polyurethane composite may have a fiber shape and / or a spherical shape.

4. The polyurethane composite material according to claim 3, characterized in that: When the polyurethane composite is in a fibrous shape, the diameter of the polyurethane composite is 100 to 150 μm.

5. The polyurethane composite material according to claim 1, characterized in that: The mass ratio of the polyurethane matrix to the polyurethane composite is 4 to 99:

1.

6. The polyurethane composite material according to claim 1, characterized in that: The melting temperature of the hard polyurethane is 20-40° C. higher than the melting temperature of the soft polyurethane.

7. A method for preparing a polyurethane foam material, characterized in that: The following steps are involved: The polyurethane composite material according to any one of claims 1 to 6 is saturated in a CO2 environment and then pressure-released for foaming to obtain the polyurethane foam material.

8. The preparation method according to claim 7, characterized in that: The saturation temperature is 10-40° C. lower than the melting temperature of the soft polyurethane in the polyurethane composite material.

9. The polyurethane foam material prepared by the preparation method according to claim 7 or 8, characterized in that: The invention has a bimodal pore structure; the average pore diameter of small pores in the bimodal pore structure is 0.4-2.5 μm, and the average pore diameter of large pores is 20-40 μm.

10. Use of the polyurethane foam material according to claim 9 in the fields of shoe materials, electromagnetic shielding materials, polishing pads or flexible sensors.

Citation Information

Patent Citations

  • Polyurethane soft foam composite material and production technology thereof

    CN105440650A

  • Thermoplastic polyurethane fiber composite material, and preparation method and application thereof

    CN107033580A

  • Surface material of urethane resin and a method for preparation thereof

    US20030087084A1

  • Shoe member and shoe

    US20230000205A1