Microcapsule revulcanized asphalt and preparation method thereof
Through the microcapsule revulcanization asphalt technology, vulcanization reaction between vulcanizing agent and rubber powder in asphalt is solved, and the effect of improving the road performance of asphalt mixture is achieved.
Patent Information
- Application Number
- CN202411334948.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-12-03
AI Technical Summary
When the existing rubber-modified asphalt increases the rubber dosage, the road performance of rubber-modified asphalt is easily reduced, and it is difficult to maintain stable performance while improving the compatibility of rubber and asphalt.
Using microcapsule re-vulcanization asphalt technology, the vulcanization agent is coated in the microcapsule, and the pressure release of the construction machinery makes it vulcanized with the rubber powder, realizing the reconstruction of the rubber powder network, thereby improving the road performance of the asphalt mixture .
It effectively improves the various road performances of asphalt mixture, avoids the performance reduction caused by rubber cracking, desulfurization, and has low viscosity and good construction ease.
Smart Images

Figure CN119060552A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of modified asphalt, and in particular to a microcapsule resulfurized asphalt and a preparation method thereof. Background Art
[0002] Rubber modified asphalt has the characteristics of high viscosity and high elasticity, and has the ability to resist fatigue cracks and reflective cracks on the road surface. The use of rubber modified asphalt can reduce the temperature sensitivity of the road surface, and under certain conditions, it can also reduce the thickness of the road surface. It also has obvious advantages in reducing noise, anti-glare and waterproof fog. At present, the method to increase the amount of rubber in rubber modified asphalt is to crack and desulfurize the waste rubber. The common methods are chemical desulfurization and physical desulfurization. In terms of chemistry, high temperature heating and high temperature pressure are used to induce changes in the cross-linking network points, and the addition of chemical additives further accelerates the speed of cracking of the cross-linking network points, so that the breaking point is stable, thereby realizing rubber regeneration. In terms of physics, it is mainly through external energy such as microwaves, ultrasound, infrared irradiation, extrusion or high shear that the three-dimensional cross-linking network points are cut off, so that the macromolecular rubber is converted into small molecular weight fragments. The molecular weight of the cracked rubber is reduced, the compatibility with asphalt is increased, and the amount of rubber in asphalt is greatly increased. However, rubber and asphalt are in a state of physical blending. The reduction in molecular weight reduces the mechanical properties of rubber while also reducing the performance of rubber modified asphalt. How to improve the compatibility between rubber and asphalt while minimizing the reduction in the road performance of rubber-modified asphalt is a difficult problem that needs to be solved urgently for rubber-modified asphalt. Summary of the invention
[0003] In order to solve the above technical problems, the purpose of the present invention is to provide a microcapsule re-sulfurized asphalt and a preparation method thereof, wherein the asphalt can release the vulcanizing agent in the microcapsule under the pressure of the construction machinery, undergo a vulcanization reaction with the rubber powder in the asphalt mixture, and achieve network reconstruction of the rubber powder, thereby improving various road performance of the asphalt mixture, solving the problem of reduced road performance of rubber modified asphalt caused by rubber cracking and desulfurization for increasing the rubber content in rubber modified asphalt.
[0004] The technical solution of the present invention to solve the above technical problems is as follows: a method for preparing microcapsule resulfurized asphalt is provided, comprising the following steps:
[0005] (1) urea, melamine and formaldehyde are stirred and mixed, triethanolamine is added to adjust the pH to 8-9, and then stirring is continued to obtain a prepolymer solution;
[0006] (2) adding a surfactant to the vulcanizing agent and stirring and emulsifying to obtain a vulcanizing agent suspension;
[0007] (3) adding the prepolymer solution obtained in step (1) to the vulcanizing agent suspension obtained in step (2) with stirring, adjusting the pH to 2-4 with dilute hydrochloric acid, and then stirring at 60-80° C. and 300-700 r / min for 1-5 hours, cooling to room temperature, filtering and drying to obtain re-vulcanized microcapsules;
[0008] (4) The road asphalt is heated to 180-190°C, SBS and desulfurized rubber powder are added, and then sheared at 4000 r / min and 180-190°C for 60-90 min, and then placed in an oven at 140-180°C for development for 1-3 h. Finally, the resulfurized microcapsules obtained in step (3) are added, and stirred at 180°C for 30 minutes to obtain microcapsule resulfurized asphalt.
[0009] Furthermore, in step (1), the molar ratio of urea, melamine and formaldehyde is 5:2-4:16-22.
[0010] Furthermore, in step (2), the vulcanizing agent is a combination of zinc oxide, zinc diethyldithiocarbamate, potassium ethyl xanthate and sulfur.
[0011] Furthermore, in step (2), the mass ratio of zinc oxide, zinc diethyldithiocarbamate, potassium ethyl xanthate and sulfur in the vulcanizing agent is 5:0.5:0.5:3-12.
[0012] Furthermore, in step (2), the surfactant is sodium dodecylbenzene sulfonate; and the mass volume concentration of the surfactant in the sulfiding agent suspension is 0-0.16%.
[0013] Furthermore, in step (2), the emulsification is stirred at a speed of 4000-6000 r / min for 10-40 min.
[0014] Furthermore, in step (3), the mass ratio of the vulcanizing agent in the vulcanizing agent suspension to the prepolymer solution is 0.6-1.2:1.
[0015] Furthermore, in step (3), the drying method is to place it in a ventilated environment and allow it to dry naturally for 1-2 days.
[0016] Furthermore, in step (4), the desulfurized rubber powder is obtained by desulfurizing rubber powder.
[0017] Furthermore, in step (4), the mass ratio of desulfurized rubber powder, SBS and road asphalt is 18-50:1-3:100; and the mass ratio of resulfurized microcapsules and desulfurized rubber powder is 5-15:100.
[0018] The present invention also provides microcapsule resulfurized asphalt prepared by the preparation method of the microcapsule resulfurized asphalt.
[0019] The beneficial effects of the scheme of the present invention are as follows: urea and melamine react with formaldehyde aqueous solution under weak alkaline conditions (PH=8-9) to generate hydroxymethyl urea groups, and then undergo polymerization in an acidic environment to form urea-formaldehyde resin with a cross-linked network structure. At the same time, the molecules of melamine interact with the molecules of urea-formaldehyde resin and are embedded in the urea-formaldehyde resin structure to form melamine-modified urea-formaldehyde resin microcapsules, thereby encapsulating the vulcanizing agent therein to form re-vulcanized microcapsules with thermal stability and reprocessing performance. Finally, a desulfurized rubber SBS composite modified asphalt is prepared, and the re-vulcanized microcapsules are added thereto to obtain microcapsule re-vulcanized asphalt.
[0020] The present invention has the following beneficial effects:
[0021] 1. The method of the present invention uses zinc oxide, sulfur, zinc diethyldithiocarbamate and potassium xanthate as vulcanizing agents, and encapsulates the rubber vulcanizing agent through microencapsulation technology, thereby ensuring that the desulfurized rubber powder and the vulcanizing agent are separated by microcapsules in the asphalt, avoiding the desulfurized rubber powder from being vulcanized during the mixing and paving of the asphalt mixture, so that the microcapsule re-sulfurized asphalt has the characteristics of lower viscosity and good ease of construction.
[0022] 2. During the pavement construction and rolling process, the microcapsule resulfurized asphalt of the present invention releases the vulcanizing agent in the microcapsules through the pressure of the construction machinery, causing it to undergo a vulcanization reaction with the rubber powder in the asphalt mixture, thereby achieving network reconstruction of the rubber powder, thereby improving various road properties of the asphalt mixture, solving the problem of reduced road performance of rubber modified asphalt caused by rubber cracking and desulfurization for increasing the rubber content in rubber modified asphalt. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is the thermogravimetric analysis diagram of the core material and the re-cured microcapsules in Experimental Example 1. DETAILED DESCRIPTION
[0024] The principles and features of the present invention are described below. The examples are only used to explain the present invention and are not used to limit the scope of the present invention. If the specific conditions are not specified in the embodiments, they are carried out according to the normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially. In the following embodiments, road asphalt uses A-90 road petroleum asphalt.
[0025] Example 1
[0026] A microcapsule resulfurized asphalt, the preparation method of which comprises the following steps:
[0027] (1) urea, melamine and formaldehyde are mixed in a molar ratio of 5:2:16, triethanolamine is added to adjust the pH to 8, and then stirring is continued to obtain a prepolymer solution;
[0028] (2) mixing the vulcanizing agent zinc oxide, zinc diethyldithiocarbamate, potassium ethyl xanthate and sulfur in a mass ratio of 5:0.5:0.5:3, adding 0.01-0.16% sodium dodecylbenzene sulfonate, stirring and emulsifying at a speed of 4000 r / min for 10 minutes to obtain a vulcanizing agent suspension;
[0029] (3) adding the prepolymer solution obtained in step (1) to the vulcanizing agent suspension obtained in step (2) with stirring, adjusting the pH to 2 with dilute hydrochloric acid, and then stirring at 60° C. and 300 r / min for 1 hour, cooling to room temperature, filtering and drying to obtain re-vulcanized microcapsules; wherein the mass ratio of the vulcanizing agent to the prepolymer solution in the vulcanizing agent suspension is 0.6:1;
[0030] (4) The road asphalt is heated to 180°C, SBS and desulfurized rubber powder are added, and then sheared at 4000 r / min and 180°C for 60 minutes, and then placed in a 140°C oven for development for 1 hour, and finally the resulfurized microcapsules obtained in step (3) are added, and stirred at 180°C for 30 minutes to obtain microcapsule resulfurized asphalt; wherein the mass ratio of desulfurized rubber powder, SBS and road asphalt is 18:1:100; and the mass ratio of resulfurized microcapsules to desulfurized rubber powder is 5:100.
[0031] Example 2
[0032] A microcapsule resulfurized asphalt, the preparation method of which comprises the following steps:
[0033] (1) urea, melamine and formaldehyde are mixed in a molar ratio of 5:4:22, triethanolamine is added to adjust the pH to 9, and then stirring is continued to obtain a prepolymer solution;
[0034] (2) mixing the vulcanizing agent zinc oxide, zinc diethyldithiocarbamate, potassium ethyl xanthate and sulfur in a mass ratio of 5:0.5:0.5:12, adding 0.16% of the surfactant sodium dodecylbenzene sulfonate, stirring and emulsifying at a speed of 6000 r / min for 40 minutes, and obtaining a vulcanizing agent suspension;
[0035] (3) adding the prepolymer solution obtained in step (1) to the vulcanizing agent suspension obtained in step (2) with stirring, adjusting the pH to 4 with dilute hydrochloric acid, and then stirring at 80° C. and 700 r / min for 5 hours, cooling to room temperature, filtering and drying to obtain re-vulcanized microcapsules; wherein the mass ratio of the vulcanizing agent to the prepolymer solution in the vulcanizing agent suspension is 1.2:1;
[0036] (4) The road asphalt is heated to 190°C, SBS and desulfurized rubber powder are added, and then sheared at 4000 r / min and 190°C for 90 minutes, and then placed in an oven at 180°C for development for 3 hours, and finally the resulfurized microcapsules obtained in step (3) are added, and stirred at 180°C for 30 minutes to obtain microcapsule resulfurized asphalt; wherein the mass ratio of desulfurized rubber powder, SBS and road asphalt is 50:3:100; and the mass ratio of resulfurized microcapsules and desulfurized rubber powder is 15:100.
[0037] Example 3
[0038] A microcapsule resulfurized asphalt, the preparation method of which comprises the following steps:
[0039] (1) urea, melamine and formaldehyde are mixed in a molar ratio of 5:3:19, triethanolamine is added to adjust the pH to 8.5, and then stirring is continued to obtain a prepolymer solution;
[0040] (2) mixing the vulcanizing agent zinc oxide, zinc diethyldithiocarbamate, potassium ethyl xanthate and sulfur in a mass ratio of 5:0.5:0.5:6, adding 0.12% of the surfactant sodium dodecylbenzene sulfonate, stirring and emulsifying at a speed of 5000 r / min for 30 minutes, and obtaining a vulcanizing agent suspension;
[0041] (3) adding the prepolymer solution obtained in step (1) to the vulcanizing agent suspension obtained in step (2) with stirring, adjusting the pH to 3 with dilute hydrochloric acid, and then stirring at 70° C. and 500 r / min for 3 hours, cooling to room temperature, filtering and drying to obtain re-vulcanized microcapsules; wherein the mass ratio of the vulcanizing agent to the prepolymer solution in the vulcanizing agent suspension is 0.6:1;
[0042] (4) The road asphalt is heated to 185°C, SBS and desulfurized rubber powder are added, and then sheared at 4000 r / min and 185°C for 70 minutes, and then placed in a 160°C oven for development for 2 hours, and finally the resulfurized microcapsules obtained in step (3) are added, and stirred at 180°C for 30 minutes to obtain microcapsule resulfurized asphalt; wherein the mass ratio of desulfurized rubber powder, SBS and road asphalt is 18:2:100; and the mass ratio of resulfurized microcapsules to desulfurized rubber powder is 7.4:100.
[0043] Comparative Example 1
[0044] 18% ordinary rubber powder-2% SBS composite modified asphalt, including ordinary rubber powder, SBS and road asphalt; the mass ratio of ordinary rubber powder, SBS and road asphalt is 18:2:100
[0045] Comparative Example 2
[0046] 18% desulfurized rubber powder-2% SBS composite modified asphalt, including desulfurized rubber powder, SBS and road asphalt; the mass ratio of desulfurized rubber powder, SBS and road asphalt is 18:2:100
[0047] Test Example 1
[0048] (1) Preparation of resulfurized microcapsules
[0049] Through single factor experiments, the effects of surfactant concentration and core-to-wall ratio on the preparation of resulfurized microcapsules were explored. The results are shown in Table 1.
[0050] Table 1 Effects of different factors on the preparation of resulfurized microcapsules
[0051]
[0052] As shown in Table 1, with the increase of surfactant concentration, the particle size changes gradually decreases first and then increases gradually, and reaches the minimum value of 42.16μm when the surfactant concentration is 0.12%. The coverage rate of re-cured microcapsules shows a trend of gradually increasing with the increase of surfactant concentration, and the maximum coverage rate is 83.65% when the surfactant concentration is 0.16%. At the same time, with the change of core-to-wall ratio, the particle size change trend of re-cured microcapsules is not obvious, while its coverage rate shows a trend of increasing first and then decreasing, reaching the maximum value of 81.67% when the core-to-wall ratio is 1:1. The smaller the particle size of the microcapsule, the better the dispersion of the re-cured microcapsules in space, and the better the vulcanization effect on the vulcanization object; the greater the coverage rate of the re-cured microcapsules, the less wall material mass is required, and the better the economy. In summary, the preparation process of resulfurized microcapsules is as follows: the concentration of surfactant is 0.12%, the core-to-wall ratio is 1:1, and the particle size of the resulfurized microcapsules is 42-45 μm, and the coverage rate is 80-82%.
[0053] (2) Analysis of thermal stability of resulfurized microcapsules
[0054] The application of resulfurized microcapsules in asphalt projects needs to ensure that they do not break during the preparation of modified asphalt, so the vulcanized microcapsules need to have a certain thermal stability. The thermal stability of the resulfurized microcapsules was analyzed using a thermogravimetric analyzer. The results are as follows: Figure 1 shown.
[0055] Depend on Figure 1 It can be seen that the thermal decomposition temperature of the re-sulfurized microcapsules is greater than the thermal decomposition temperature of the core material, and has good thermal stability within the temperature of 200°C. Based on this, it can be judged that during the processing of modified asphalt, the sulfurized microcapsules will not cause the core material to rupture due to high temperature.
[0056] Test Example 2
[0057] Different proportions of sulfur were added to 18% desulfurized rubber powder-2% SBS composite modified asphalt to obtain resulfurized rubber powder-SBS composite modified asphalt containing different sulfur addition ratios, and then the performance was compared with the asphalt of comparative examples 1 and 2. The results are shown in Table 2.
[0058] Table 2 Comparison of different asphalt properties
[0059]
[0060] As shown in Table 2, after being modified by a vulcanizing agent (sulfur), the penetration of the desulfurized rubber powder composite modified asphalt is significantly reduced, and the softening point is significantly increased. The 5°C elongation and elastic recovery modulus first increase and then decrease with the increase of sulfur content, reaching a maximum value when the content reaches 6% (ratio of rubber mass), and then when the content is greater than 6%, the elongation of the modified asphalt begins to decrease, and when the sulfur content is greater than 9%, it decreases significantly. In summary, the optimal sulfur content in the 18% desulfurized rubber powder-2% SBS composite modified asphalt is 6%, and the corresponding content of resulfurized microcapsules in the desulfurized rubber powder composite modified asphalt is 14.8%. At the same time, it can be found in the study of microcapsule resulfurized asphalt that its performance is basically similar to that of Comparative Example 2, from which it can be seen that the microcapsules can effectively isolate the contact between the core material and the desulfurized rubber powder during the preparation of the modified asphalt.
[0061] Test Example 3
[0062] The Shaanxi local standard DB 61 / T 1021-2016 Technical Specification for Rubber Asphalt Pavement Construction is adopted, and the rubber asphalt mixture mineral aggregate grading is carried out according to the ARG-13 mixture proportion requirements in Table 3.
[0063] Table 3 ARG-13 mixture proportion
[0064]
[0065] (1) The test results of various indicators of 18% desulfurized rubber powder-2% SBS composite modified asphalt mixture with different asphalt-stone ratios are shown in Table 4.
[0066] Table 4 Test results of various indicators of rubber asphalt mixture
[0067] Oil-stone ratio (%) 5.0 5.5 6.0 6.5 7.0 Gross volume relative density 2.462 2.474 2.483 2.478 2.471 Void ratio (%) 5.8 4.8 3.8 3.4 3.0 Clearance ratio (%) 16.47 16.50 16.64 17.25 17.89 Saturation (%) 64.52 71.12 77.13 80.34 83.09 Stability (kN) 9.51 10.22 9.97 9.74 9.48 Flow value(mm) 2.9 3.3 3.6 4.0 4.4
[0068] From the data analysis in Table 4, it can be seen that OAC1=5.82%, OAC2=5.95%, and OAC=5.89%.
[0069] Therefore, the optimal oil-to-stone ratio of 18% desulfurized rubber powder-2% SBS composite modified asphalt and microcapsule resulfurized asphalt is 5.89; similarly, the optimal oil-to-stone ratio of 18% ordinary rubber powder-2% SBS composite modified asphalt is 6.18; the optimal oil-to-stone ratio of matrix asphalt composite modified asphalt is 5.12; and the optimal oil-to-stone ratio of 2% SBS composite modified asphalt is 5.57.
[0070] (2) High temperature performance of rubber asphalt mixture
[0071] According to the specifications, the rutting specimens of the asphalt mixture were prepared by a rutting plate former according to the oil-stone ratio of the above asphalt mixture, and then the high stability of the mixture was tested by a rutting tester. The dynamic stability of different types of asphalt mixtures is shown in Table 5.
[0072] Table 5 Dynamic stability data of different types of asphalt mixtures
[0073]
[0074] As shown in Table 5, after adding SBS to the base asphalt, the dynamic stability of the asphalt is slightly improved; after adding ordinary rubber, the SBS and rubber in the SBS modified asphalt are cross-linked to form a more stable cross-linked structure, which significantly increases its dynamic stability; after the rubber in the composite modified asphalt is desulfurized, its dynamic stability decreases from 4805 times / mm to 3380 times / mm. This is because after the rubber is desulfurized, its CS bond is broken, the molecular weight is reduced, and the viscosity is reduced, which reduces the adhesion of the composite modified asphalt and significantly reduces the high temperature performance. After the desulfurized rubber composite modified asphalt is added with the resulfurized microcapsules, the capsule wall of the resulfurized microcapsules is broken under the action of mechanical pressure, and the vulcanizing agent is released to contact with the desulfurized rubber, and the desulfurized rubber is resulfurized, which increases the molecular weight and adhesion of the desulfurized rubber, improves the dynamic stability of the composite modified asphalt, and improves its high temperature performance.
[0075] (3) Low temperature performance of rubber asphalt mixture
[0076] The results of low-temperature beam bending tests on different types of asphalt mixtures are shown in Table 6.
[0077] Table 6 Results of low temperature beam bending tests on different types of asphalt mixtures
[0078]
[0079] As shown in Table 6, the maximum flexural strain of the composite modified asphalt is greater than that of the SBS modified asphalt. This is because the damage process of the two is different: on the one hand, the crack development of the rubber powder modified asphalt mixture will start from the fine shear band and gradually expand. This process will consume external energy, so that it can withstand greater deformation, and the low-temperature performance is improved; on the other hand, after the rubber powder and SBS are composite modified, the internal network structure of the binder is denser and the cohesion is improved, so their mixture has better low-temperature performance. After the rubber is desulfurized, the molecular weight between rubbers is reduced, and the degree of crosslinking is reduced after swelling in asphalt, which also reduces the low-temperature performance of the composite modified asphalt. The maximum flexural strain of the microcapsule resulfurized asphalt with resulfurized microcapsules is restored to the level of the undesulfurized composite modified asphalt. This is because the desulfurized rubber after swelling reacts chemically with the vulcanizing agent, which increases the degree of crosslinking between rubbers and increases the low-temperature performance of asphalt.
[0080] (4) Water stability of asphalt mixture
[0081] Table 7 Test results of water stability of different types of asphalt mixtures
[0082]
[0083] As shown in Table 7, after adding SBS modifier to road asphalt, its stability is significantly increased, and its water stability is better; compared with SBS modified asphalt, the residual stability of the composite modified asphalt with waste rubber powder is greater. This is because after adding waste rubber powder to asphalt with low SBS dosage, SBS uses the swollen waste rubber powder as an anchor point to form a more stable network cross-linked structure in the asphalt, which has stronger water stability; after desulfurization, the molecular weight of the waste rubber powder is reduced, resulting in a decrease in the degree of cross-linking between molecules after swelling, which will reduce the water stability of the composite modified asphalt and make its residual stability lower than that of the non-desulfurized composite modified asphalt; in the composite modified asphalt after adding microcapsules, after the microcapsules are broken, the vulcanizing agent contained in them will react with the desulfurized rubber to undergo a vulcanization reaction, so that the swollen desulfurized waste rubber powder has a denser cross-linked structure, which improves its residual stability and improves its water stability.
[0084] (5) Freeze-thaw splitting of asphalt mixture
[0085] Table 8 Results of freeze-thaw splitting tests on different types of asphalt mixtures
[0086]
[0087] It can be seen from Table 8 that, similar to the results of the submerged Marshall stability test, the addition of SBS modifier increases the TSR of the base asphalt, improves the water damage resistance and low-temperature performance of the asphalt mixture; the addition of waste rubber powder improves the TSR of low-dosage SBS modified asphalt to a certain extent; the TSR of the desulfurized composite modified asphalt is lower than that of the non-desulfurized composite modified asphalt to a certain extent, and the TSR of the microcapsule resulfurized asphalt after adding microcapsules is not much different from the TSR of the non-desulfurized composite modified asphalt, and its resistance to low-temperature water damage is significantly improved compared with the desulfurized composite modified asphalt.
[0088] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing microcapsule resulfurized asphalt, characterized in that: The following steps are involved: (1) urea, melamine and formaldehyde are stirred and mixed, triethanolamine is added to adjust the pH to 8-9, and then stirring is continued to obtain a prepolymer solution; (2) adding a surfactant to the vulcanizing agent and stirring and emulsifying to obtain a vulcanizing agent suspension; (3) adding the prepolymer solution obtained in step (1) to the vulcanizing agent suspension obtained in step (2) with stirring, adjusting the pH to 2-4 with dilute hydrochloric acid, and then stirring at 60-80° C. and 300-700 r / min for 1-5 hours, cooling to room temperature, filtering and drying to obtain re-vulcanized microcapsules; (4) The road asphalt is heated to 180-190°C, SBS and desulfurized rubber powder are added, and then sheared at 4000 r / min and 180-190°C for 60-90 min, and then placed in an oven at 140-180°C for development for 1-3 h. Finally, the resulfurized microcapsules obtained in step (3) are added, and stirred at 180°C for 30 minutes to obtain microcapsule resulfurized asphalt.
2. The method for preparing microcapsule resulfurized asphalt according to claim 1, characterized in that: In step (1), the molar ratio of urea, melamine and formaldehyde is 5:2-4:16-22.
3. The method for preparing microcapsule resulfurized asphalt according to claim 1, characterized in that: In step (2), the vulcanizing agent is a composition of zinc oxide, zinc diethyldithiocarbamate, potassium ethyl xanthate and sulfur.
4. The method for preparing microcapsule resulfurized asphalt according to claim 3, characterized in that: In step (2), the mass ratio of zinc oxide, zinc diethyldithiocarbamate, potassium ethyl xanthate and sulfur in the vulcanizing agent is 5:0.5:0.5:3-12.
5. The method for preparing microcapsule resulfurized asphalt according to claim 1, characterized in that: In step (2), the surfactant is sodium dodecylbenzene sulfonate; and the mass volume concentration of the surfactant in the sulfiding agent suspension is 0-0.16%.
6. The method for preparing microcapsule resulfurized asphalt according to claim 1, characterized in that: In step (3), the mass ratio of the vulcanizing agent to the prepolymer solution in the vulcanizing agent suspension is 0.6-1.2:
1.
7. The method for preparing microcapsule resulfurized asphalt according to claim 1, characterized in that: In step (4), the desulfurized rubber powder is obtained by desulfurizing rubber powder.
8. The method for preparing microcapsule resulfurized asphalt according to claim 1, characterized in that: In step (4), the mass ratio of the desulfurized rubber powder, SBS and road asphalt is 18-50:1-3:100; the mass ratio of the resulfurized microcapsules and the desulfurized rubber powder is 5-15:
100.
9. Microcapsule resulfurized asphalt prepared by the method for preparing microcapsule resulfurized asphalt according to any one of claims 1 to 8.