Crude oil of self-adhesive waterproof coiled material, self-adhesive waterproof coiled material and preparation method of self-adhesive waterproof coiled material
By using self-adhesive waterproof coil crude oil formula and specific processing technology in waterproof coils, the problem of insufficient adhesion and durability of traditional waterproof coils is solved, and the tensile resistance and waterproof effect is improved, and the simplification of the simplification The construction process is carried out and the risk of water leakage is reduced.
Patent Information
- Application Number
- CN202411300851.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional waterproof coils have problems such as poor adhesion and poor durability during construction and use, which leads to increased construction complexity and cost, and are prone to cracks and water leakage.
Using self-adhesive waterproof coil crude oil formula, including asphalt, styrene butadiene-styrene block copolymer, asphalt base oil, resin, glue powder and talc, through specific mixing and processing processes A self-adhesive waterproof coil with good tensile resistance is formed, and coated and coated on the dry nonwoven fabric to improve adhesion.
It significantly improves the tensile resistance and waterproof effect of self-adhesive waterproof coils, reduces the generation of cracks, ensures stability in high and low temperature environments, simplifies the construction process, and achieves rapid and firm bonding through hot melting machines. , improves waterproofing effect.
Smart Images

Figure CN119060688A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building waterproof materials, and in particular relates to a self-adhesive waterproof coiled material crude oil and a self-adhesive waterproof coiled material and a preparation method thereof. Background Art
[0002] With the development of my country's economic construction and social progress, people's living standards are constantly improving, and the requirements for living environment are getting higher and higher. The quality of waterproofing projects is particularly important. The quality of waterproofing projects directly affects the performance and service life of buildings. At present, there are many kinds of waterproof materials sold on the market, among which waterproof coatings are the mainstream products, but waterproof coatings have the disadvantages of complex construction, low efficiency and high cost. Waterproof membranes have the advantages of convenient and fast construction, and are more and more widely used in waterproofing projects.
[0003] Although traditional waterproof membranes have a certain waterproof effect, they still have some shortcomings during construction and use, such as weak adhesion and low durability. In order to improve the overall performance of waterproof membranes, it is particularly important to develop new self-adhesive waterproof membranes. At present, waterproof membranes usually use asphalt, rubber and other materials as substrates to improve their waterproof effect. Or they can enhance their waterproof performance by coating waterproof coatings on the substrate or adding other materials. However, these materials may require additional adhesives during construction, which increases the complexity and cost of construction. Self-adhesive waterproof membranes achieve waterproof effects by adding a self-adhesive layer to the substrate, but the adhesion and durability of the self-adhesive layer still need to be improved. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a self-adhesive waterproof coiled material and a self-adhesive waterproof coiled material and a preparation method thereof, and provides a self-adhesive waterproof coiled material with good tensile resistance and excellent waterproof effect.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:
[0006] A self-adhesive waterproof coiled material crude oil comprises the following raw materials in parts by weight: 36-38 parts of asphalt, 3-4 parts of styrene-butadiene rubber, 2-4 parts of styrene-butadiene-styrene block copolymer, 9-20 parts of asphalt base oil, 1-2 parts of resin, 4-19 parts of rubber powder and 24-32 parts of talcum powder.
[0007] Preferably, the asphalt base oil is cycloalkane oil.
[0008] The resin includes one or more of polyester resin, acrylic resin and epoxy resin.
[0009] The rubber powder includes one or both of tire recycled rubber powder and asphalt modified rubber powder.
[0010] The present invention also provides a self-adhesive waterproof coiled material, comprising a dried non-woven fabric, a coating material and the self-adhesive waterproof coiled material raw material, the self-adhesive waterproof coiled material raw material is soaked in the lower surface of the dried non-woven fabric and coated on the upper surface of the dried non-woven fabric, and the upper and lower surfaces of the dried non-woven fabric are bonded to the coating material through the self-adhesive waterproof coiled material raw material.
[0011] Preferably, the coating material includes one or more of PE film, fine sand, and mineral granules.
[0012] The present invention also provides a method for preparing a self-adhesive waterproof membrane, comprising the following steps:
[0013] S1. Weigh asphalt and asphalt base oil by weight, mix and stir the two, add styrene-butadiene rubber and styrene-butadiene-styrene block copolymer, heat to a certain temperature, and keep dissolving at this temperature for 2 hours to obtain a mixture A;
[0014] S2, adding resin and rubber powder to mixture A, heating to a certain temperature, and maintaining the dissolution and modification at this temperature for 2 hours to obtain mixture B;
[0015] S3, grinding the mixture B, pouring it back after grinding, adding talcum powder in batches, stirring it thoroughly, and obtaining a self-adhesive waterproofing coiled material crude oil;
[0016] S4, soaking the crude oil of the self-adhesive waterproof coiled material obtained in step S3 on the lower surface of the dried non-woven fabric, coating it on the upper surface of the dried non-woven fabric, laminating the upper and lower surfaces of the treated non-woven fabric, and rolling the formed material through a cooling facility, cooling it to room temperature, and then rolling it up to obtain the self-adhesive waterproof coiled material.
[0017] Preferably, after adding styrene-butadiene rubber and styrene-butadiene-styrene block copolymer in step S1, the temperature is raised to 190-200°C.
[0018] Preferably, after adding resin and rubber powder to mixture A in step S2, the temperature is raised to 205-215°C.
[0019] Preferably, in step S3, the mixture B is ground at a temperature of 190-210° C. and a grinding time of 60-80 min.
[0020] Preferably, in step S3, talcum powder is added in batches at a temperature not lower than 185° C. and stirred for more than 60 minutes to obtain a self-adhesive waterproofing membrane crude oil.
[0021] Preferably, in step S4, the self-adhesive waterproof coiled material crude oil is immersed on the lower surface of the dried non-woven fabric at 170-190°C.
[0022] Preferably, in step S4, the self-adhesive waterproof coiled material crude oil is coated on the upper surface of the dried non-woven fabric at 165-185°C.
[0023] Preferably, during the roller forming process, the self-adhesive waterproof membrane with a thickness of 3-4 mm is prepared by adjusting the roller height.
[0024] Compared with the prior art, the present invention has the following advantages and technical effects:
[0025] 1. The self-adhesive waterproof membrane provided by the present invention has strong tensile strength. Compared with the traditional waterproof membrane that is prone to cracks at the joints, resulting in technical problems such as water leakage, the self-adhesive waterproof membrane of the present invention significantly improves the tensile strength, so that the membrane can remain stable in high and low temperature environments and has good adhesion, thereby reducing or even eliminating the occurrence of cracks and effectively avoiding water leakage.
[0026] 2. The self-adhesive waterproof membrane of the present invention is suitable for waterproofing of roofs, basements and other parts, and has an excellent waterproofing effect, meeting strict building waterproofing requirements.
[0027] 3. The self-adhesive waterproofing membrane of the present invention is easy and efficient to lay when in use. By using a hot melt machine to connect the joints between the membranes, fast and firm bonding can be achieved. Not only is the operation easy, but the sealing between the membranes can also be ensured, further improving the waterproofing effect. In addition, the self-adhesive waterproofing membrane of the present invention can be embossed by embossing the self-adhesive waterproofing membrane according to actual needs.
[0028] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a process flow chart of the self-adhesive waterproof membrane prepared in Example 1. DETAILED DESCRIPTION
[0030] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.
[0031] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one having ordinary skills in the field to which the present invention belongs.
[0032] Asphalt 70# used in the embodiments of the present invention was purchased from Hebei Xinhai Chemical Group Co., Ltd.; styrene-butadiene rubber SBR was purchased from Shandong Gaoshi Science and Technology Industry and Trade Co., Ltd.; styrene-butadiene-styrene block copolymer SBS (161B) was purchased from Beijing Yanshan Petrochemical Company; asphalt base oil was purchased from Cangzhou Huaze Chemical Co., Ltd.; resin was purchased from Wenan County Yubo Trading Co., Ltd.; rubber powder was purchased from Hebei Zeyuan Rubber Co., Ltd.; talcum powder was purchased from Wuqiao Haoyue Building Materials Sales Co., Ltd.
[0033] Example 1
[0034] Weigh 3680 kg of 70# asphalt and 1922 kg of cycloalkyl oil, mix them thoroughly and stir them evenly, add 325 kg of SBR and 350 kg of SBS (model 161B) into a closed insulated batching tank, heat it to 195°C, and continue dissolving at this temperature for 2 hours to obtain mixture A.
[0035] S2, adding 200 kg of polyester resin and 978 kg of tire recycled rubber powder to mixture A, heating to 215° C., and maintaining the dissolution modification at this temperature for 2 hours to obtain mixture B;
[0036] S3, the mixture B flows into the colloid mill for grinding treatment, the grinding temperature is 190 ° C, the grinding time is 60 min, after grinding, it is poured back into the mixing tank, 2549 kg of talcum powder is added in batches at 190 ° C, and it is fully stirred for 80 min to obtain the self-adhesive waterproofing coiled material crude oil, which flows into the oil immersion tank;
[0037] S4. Immerse the self-adhesive waterproofing membrane crude oil on the lower surface of the dried non-woven fabric in an oil immersion pool at 180°C, transfer to an oil coating pool, and coat the self-adhesive waterproofing membrane crude oil on the upper surface of the dried non-woven fabric in an oil coating pool at 175°C. The treated upper and lower surfaces of the non-woven fabric are coated, wherein the coating material is PE film and fine sand, which are roll-formed, and the formed material passes through a cooling facility, and is rolled up after being cooled to room temperature to obtain a self-adhesive waterproofing membrane.
[0038] Example 2
[0039] S1. Weigh 4675 kg of 70# asphalt and 1225 kg of naphthenic oil, mix and stir them evenly, add 475 kg of SBR and 300 kg of SBS (161B), add them into a closed heat-insulated batching tank, heat to 195° C., and keep them dissolved at this temperature for 2 hours to obtain a mixture A;
[0040] S2, adding 200 kg of acrylic resin and 1650 kg of asphalt modified rubber powder to mixture A, raising the temperature to 215° C., and maintaining the dissolution and modification at this temperature for 2 hours to obtain mixture B;
[0041] S3, the mixture B is flowed into the colloid mill for grinding treatment, the grinding temperature is 190 ° C, the grinding time is 60 min, after grinding, it is poured back into the mixing tank, 3925 kg of talcum powder is added in batches at 190 ° C, and it is fully stirred for 80 min to obtain the self-adhesive waterproofing coiled material crude oil, which flows into the oil immersion tank;
[0042] S4. Immerse the self-adhesive waterproofing membrane crude oil on the lower surface of the dried non-woven fabric in an oil immersion pool at 180°C, transfer to an oil coating pool, and coat the self-adhesive waterproofing membrane crude oil on the upper surface of the dried non-woven fabric in an oil coating pool at 175°C. The treated upper and lower surfaces of the non-woven fabric are coated, wherein the coating material is PE film and fine sand, which are roll-formed, and the formed material passes through a cooling facility, and is rolled up after being cooled to room temperature to obtain a self-adhesive waterproofing membrane.
[0043] Comparative Example 1
[0044] S1. Weigh 3680 kg of 70# asphalt and 1922 kg of naphthenic oil, mix and stir them evenly, add 200 kg of SBR and 150 kg of SBS (161B), add them into a closed heat-insulated batching tank, heat to 195° C., and keep dissolving at this temperature for 2 hours to obtain a mixture A;
[0045] S2, adding 200 kg of epoxy resin and 1500 kg of tire recycled rubber powder to mixture A, raising the temperature to 215° C., and maintaining the dissolution and modification at this temperature for 2 hours to obtain mixture B;
[0046] S3, the mixture B is flowed into the colloid mill for grinding treatment, the grinding temperature is 190 ° C, the grinding time is 60 min, after grinding, it is poured back into the mixing tank, 2352 kg of talcum powder is added in batches at 190 ° C, and it is fully stirred for 80 min to obtain the self-adhesive waterproofing coiled material crude oil, which flows into the oil immersion tank;
[0047] S4. Immerse the self-adhesive waterproofing membrane crude oil on the lower surface of the dried non-woven fabric in an oil immersion pool at 180°C, transfer to an oil coating pool, and coat the self-adhesive waterproofing membrane crude oil on the upper surface of the dried non-woven fabric in an oil coating pool at 175°C. The treated upper and lower surfaces of the non-woven fabric are coated, wherein the coating material is PE film and fine sand, which are roll-formed, and the formed material passes through a cooling facility, and is rolled up after being cooled to room temperature to obtain a self-adhesive waterproofing membrane.
[0048] Comparative Example 2
[0049] S1. Weigh 4675 kg of 70# asphalt and 1000 kg of naphthenic oil, mix and stir them evenly, add 250 kg of SBR and 200 kg of SBS (161B), add them into a closed heat-insulated batching tank, heat to 195° C., and keep dissolving at this temperature for 2 hours to obtain a mixture A;
[0050] S2, adding 200 kg of acrylic resin and 1650 kg of asphalt modified rubber powder to mixture A, raising the temperature to 215° C., and maintaining the dissolution and modification at this temperature for 2 hours to obtain mixture B;
[0051] S3, the mixture B is flowed into the colloid mill for grinding, the grinding temperature is 190 ° C, the grinding time is 60 min, after grinding, it is poured back into the mixing tank, 4475 kg of talcum powder is added in batches at 190 ° C, and it is fully stirred for 80 min to obtain the self-adhesive waterproofing coiled material crude oil, which flows into the oil immersion tank;
[0052] S4. Immerse the self-adhesive waterproofing membrane crude oil on the lower surface of the dried non-woven fabric in an oil immersion pool at 180°C, transfer to an oil coating pool, and coat the self-adhesive waterproofing membrane crude oil on the upper surface of the dried non-woven fabric in an oil coating pool at 175°C. The treated upper and lower surfaces of the non-woven fabric are coated, wherein the coating material is PE film and fine sand, which are roll-formed, and the formed material passes through a cooling facility, and is rolled up after being cooled to room temperature to obtain a self-adhesive waterproofing membrane.
[0053] The effects of the self-adhesive waterproof membranes provided in the above-mentioned Examples 1-2 and Comparative Examples 1-2 were verified by the following tests:
[0054] Heat resistance test: refer to GB / T 328-2007 "Heat resistance of asphalt waterproofing membrane" for sample preparation and testing. The test results are shown in Table 1.
[0055] Average tensile test: Tested in accordance with GB / T328.8-2007 "Tensile properties of asphalt waterproofing membranes". The test results are shown in Table 1.
[0056] Waterproofness test: According to method B in GB / T 328.10-2007, a 7-hole plate is used, and the upper surface faces water. When the upper surface is fine sand or mineral granular material, the lower surface faces water. When the lower surface is also fine sand, before the test, the fine sand on the lower surface is removed along the sealing ring, and then a circle of 60-100 hot asphalt is applied. After the coating is flat and cooled for 1 hour, the water-proofness is tested. The test results are shown in Table 1.
[0057] Low temperature flexibility test: Low temperature flexibility is tested according to the method described in GB / T328.14-2007 “Low temperature flexibility of asphalt waterproofing membrane”. The test results are shown in Table 1.
[0058] Table 1 Performance test results
[0059]
[0060]
[0061] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A self-adhesive waterproofing roll material. It is characterized in that The invention comprises the following raw materials in parts by weight: 36-38 parts of asphalt, 3-4 parts of styrene-butadiene rubber, 2-4 parts of styrene-butadiene-styrene block copolymer, 9-20 parts of asphalt base oil, 1-2 parts of resin, 4-19 parts of rubber powder and 24-32 parts of talc powder.
2. A self-adhesive waterproof membrane, It is characterized in that It comprises a drying non-woven fabric, a coating material and the self-adhesive waterproof coiled material raw material according to claim 1, wherein the self-adhesive waterproof coiled material raw material is soaked in the lower surface of the drying non-woven fabric and coated on the upper surface of the drying non-woven fabric, and the upper and lower surfaces of the drying non-woven fabric are bonded to the coating material through the self-adhesive waterproof coiled material raw material.
3. A self-adhesive waterproof membrane according to claim 2, It is characterized in that The covering material includes one or more of PE film, fine sand and mineral granules.
4. A method for preparing a self-adhesive waterproof membrane as claimed in claim 2 or 3, It is characterized in that The steps include: S1. Weigh asphalt and asphalt base oil by weight, mix and stir the two, add styrene-butadiene rubber and styrene-butadiene-styrene block copolymer, heat to a certain temperature, and keep dissolving at this temperature for 2 hours to obtain a mixture A; S2, adding resin and rubber powder to mixture A, heating to a certain temperature, and maintaining the dissolution and modification at this temperature for 2 hours to obtain mixture B; S3, grinding the mixture B, pouring it back after grinding, adding talcum powder in batches, stirring it thoroughly, and obtaining a self-adhesive waterproofing coiled material crude oil; S4, soaking the crude oil of the self-adhesive waterproof coiled material obtained in step S3 on the lower surface of the dried non-woven fabric, coating it on the upper surface of the dried non-woven fabric, laminating the upper and lower surfaces of the treated non-woven fabric, and rolling the formed material through a cooling facility, cooling it to room temperature, and then rolling it up to obtain the self-adhesive waterproof coiled material.
5. The preparation method according to claim 4, It is characterized in that After adding styrene-butadiene rubber and styrene-butadiene-styrene block copolymer in step S1, the temperature is raised to 190-200°C.
6. The preparation method according to claim 4, It is characterized in that In step S2, after adding resin and rubber powder to mixture A, the temperature is raised to 205-215°C.
7. The preparation method according to claim 4, It is characterized in that In step S3, the mixture B is ground at a temperature of 190-210° C. and a grinding time of 60-80 min.
8. The preparation method according to claim 4, It is characterized in that In step S3, talcum powder is added in batches at a temperature not lower than 185° C. and stirred for more than 60 minutes to obtain a self-adhesive waterproofing coiled material crude oil.
9. The preparation method according to claim 4, It is characterized in that In step S4, at 170-190° C., the self-adhesive waterproofing coiled material crude oil is immersed on the lower surface of the dried non-woven fabric.
10. The preparation method according to claim 4, It is characterized in that In step S4, the self-adhesive waterproofing coiled material crude oil is coated on the upper surface of the dried non-woven fabric at 165-185°C.
Citation Information
Patent Citations
Self-adhesive rubber bituminous waterproof sheet material and preparation technology thereof
CN101644096A
Self-adhesion waterproof rolls used for road bridge and preparation method thereof
CN103160241A
Self-adhesive polymer modified asphalt waterproof coiled material and preparation method and application thereof
CN110204914A
Composition self adhesive asphalt waterproofing sheet waterproofing sheet manufacturing method and composite waterproof construction