Method for deeply dephosphorizing chromium-nickel pig iron melt smelted by electric furnace

Through the deep dephosphorization method of chromium nickel pig iron melting in electric furnace, the batch addition of solid and powdered dephosphorizer and oxygen blowing in is used to solve the problem of high phosphorus content in chromium nickel pig iron, and the low phosphorus and high nickel stainless steel mother liquid is achieved The production simplifies the process and reduces the smelting cost.

CN119061224AActive Publication Date: 2024-12-03SHANXI TAIGANG STAINLESS STEEL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410980574.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-12-03
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

In the prior art, chromium-nickel pig iron contains high residual elements such as P, S, Si, etc., which makes it difficult to dephosphorize in the production of low-phosphorus special stainless steel, resulting in high smelting costs and complex processes, and cannot be used in batches. In the production of low-phosphorus special stainless steel.

Method used

The deep dephosphorization method of chromium nickel pig iron melt is adopted for electric furnace melting. Through the steps of adding solid and powdered dephosphorizer in batches, blowing oxygen inlet and stirring in electric furnace, the temperature and alkalinity are controlled, and the phosphorus content is gradually reduced to reach P≤0.004. % low phosphorus high nickel stainless steel mother liquor production.

Benefits of technology

It realizes low-cost batch use of cheap chromium-nickel pig iron, simplifies production processes, reduces carbon emissions and smelting costs, avoids blast furnace dephosphorization molten iron process, and improves the smelting efficiency and economic benefits of low-phosphorus stainless steel.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for deeply dephosphorizing chromium-nickel pig iron melt smelted in an electric furnace. The method comprises the following steps: filling chromium-nickel pig iron into the electric furnace and melting the chromium-nickel pig iron into chromium-nickel pig iron pre-melt; desiliconizing and dechroming after melting down in an electric furnace, adding a solid dephosphorizing agent, supplying oxygen by a furnace door oxygen lance, and adding lime for slagging; after desilicication and dechroming are stopped, slagging off is conducted, electric furnace deep dephosphorization is conducted, a solid dephosphorizing agent is added, oxygen is continuously supplied through a furnace door oxygen lance, a powdery dephosphorizing agent is sprayed into an electric furnace carbon powder gun, and lime is added for slagging; and after deep dephosphorization of the electric furnace is completed, a furnace door oxygen lance blows nitrogen for strong stirring. The method solves the technical problem of high cost caused by the use of dephosphorized molten iron and pure nickel in stainless steel smelting due to difficulty in dephosphorizing the chromium-nickel pig iron melt in an electric furnace. The purposes that the low-phosphorus high-nickel stainless steel mother liquor is prepared through electric furnace deep dephosphorization by adopting the cheap chromium-nickel pig iron as the raw material, and the low-phosphorus special stainless steel variety is produced by matching the low-phosphorus high-nickel stainless steel mother liquor with the high-carbon ferrochrome are achieved, the production process is simplified, and the smelting cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of stainless steel production, and in particular relates to a method for deep dephosphorization of chromium-nickel pig iron melt smelted in an electric furnace. Background Art

[0002] Phosphorus is generally regarded as a harmful element in stainless steel. It has adverse effects on the surface quality, cracks, ductility, tensile strength, pitting corrosion resistance, stress corrosion resistance and welding performance of steel, especially the cold brittleness at low temperatures. Therefore, further reducing the phosphorus content in stainless steel, smelting low-phosphorus and ultra-low-phosphorus stainless steel, and improving steel performance are still one of the development trends of stainless steel production.

[0003] As a green steel material that is corrosion-resistant, beautiful and recyclable, stainless steel is increasingly used. It is widely used in some special fields such as photovoltaics, nuclear power, fine strips, welding wires, etc., which puts higher requirements on the variety and quality of stainless steel. Some steel grades require P ≤ 0.015% in the steel. Therefore, in the production process, it is necessary to use pre-treated deep dephosphorized iron water or ultra-low phosphorus scrap steel and add high-purity pure nickel (nickel plate, nickel bean) alloy, which makes the smelting process of these stainless steel varieties complicated and the manufacturing cost high.

[0004] At present, with the promotion of the process of producing chromium-nickel pig iron from laterite nickel ore through RKEF (Rotary Klin Electric Furnace), the low-priced nickel pig iron has become the main raw material of stainless steel and is widely used in the production of ordinary stainless steel, reducing the smelting cost of stainless steel. However, nickel pig iron contains relatively high residual elements such as P, S, and Si. However, since stainless steel does not have the ability to dephosphorize during smelting, cheap chromium-nickel pig iron cannot be used in large quantities for the production and smelting of low-phosphorus special stainless steel varieties. The production and smelting of low-phosphorus special stainless steel varieties can only use blast furnace dephosphorized iron water + pure nickel / high nickel iron as the main raw material, which has complex procedures and high smelting costs. Summary of the invention

[0005] In order to solve the above-mentioned technical problems existing in the prior art, the present invention has developed a method for deep dephosphorization of chromium-nickel pig iron melt smelted in an electric furnace. With cheap chromium-nickel pig iron as raw material, deep dephosphorization in an electric furnace is performed to produce a stainless steel mother liquor with low phosphorus and high nickel content of P≤0.004%, thereby achieving the purpose of using chromium-nickel pig iron raw materials in batches to produce low-phosphorus special stainless steel varieties with P≤0.015% at low cost.

[0006] The method for deep dephosphorization of chromium-nickel pig iron melt smelted in an electric furnace of the present invention comprises the following steps:

[0007] Step 1: Load chromium-nickel pig iron into an electric furnace and melt the chromium-nickel pig iron to form a chromium-nickel pig iron pre-melt;

[0008] Step 2: After the electric furnace is melted, desiliconization and dechromization operations are carried out. In this process, solid dephosphorization agent is added in batches from the high-level silo of the electric furnace for multiple times. The total amount of solid dephosphorization agent added per ton of steel is controlled to be 20-25 kg. Oxygen is supplied by the furnace door oxygen lance, and the oxygen supply flow rate per ton of steel is controlled to be 0.24-0.32 Nm 3 / min; lime is added in batches during the process, and the total amount of lime added is controlled to be 15-20kg per ton of steel, and desiliconized slag with a basicity of 1.8-2.5 is produced. During the smelting process, the electric furnace continuously supplies electrified slag to control the temperature of the molten steel in the electric furnace at 1420-1480℃;

[0009] Step 3: When Si≤0.02% and Cr≤0.80% in the molten steel, stop desiliconization and dechromization, perform electric furnace slag removal, and remove ≥70% of the desiliconization slag;

[0010] Step 4: After slagging, deep dephosphorization is carried out in the electric furnace. Solid dephosphorization agent is added from the high-level silo in batches for multiple times. The total amount of solid dephosphorization agent added per ton of steel is controlled to be 15-18 kg. The oxygen lance at the furnace door continues to supply oxygen, and the oxygen flow rate per ton of steel is controlled to be 0.30-0.38 Nm 3 / min, and at the same time, the electric furnace carbon powder gun sprays powdered dephosphorization agent, and the carrier gas for spraying the powdered dephosphorization agent is nitrogen, and the nitrogen pressure is controlled to be 1.0MPa; during the dephosphorization process, lime is added in batches from a high position, and the total amount of lime added is controlled to be 15-18kg per ton of steel, and dephosphorization slag with a basicity of 5-8 is used for deep dephosphorization. During the dephosphorization process, the electric furnace continuously supplies electrified slag to control the molten steel temperature at 1500-1550℃;

[0011] Step 5: When P in the molten steel is less than or equal to 0.004%, dephosphorization is terminated, oxygen lance at the furnace door stops blowing oxygen, and nitrogen is blown for strong stirring. The nitrogen supply flow rate per ton of steel is controlled to be 0.35-0.45Nm 3 / min, stir for 3 to 5 minutes, continue to supply power to the electric furnace to raise the temperature to above 1630℃, remove ≥80% of the dephosphorization slag, and produce low-phosphorus and high-nickel stainless steel mother liquor.

[0012] Furthermore, in the above-mentioned method for deep dephosphorization of chromium-nickel pig iron melt smelted in an electric furnace, the solid dephosphorization agent is prepared by converter dust removal ash, sintered ore and light-burned magnesium powder in a weight percentage ratio of 70:20:10, and the composition of the solid dephosphorization agent is controlled to be: FeOx: 56-70%, CaO: 10-18%, MgO: 3-8%, SiO 2 :1.5~3%.

[0013] Furthermore, in the above-mentioned method for deep dephosphorization of chromium-nickel pig iron melt in electric furnace, the powdery dephosphorization agent is composed of lime powder with CaO≥90.0%, CaF 2Fluorite powder with FeOx≥88.0% and iron oxide powder with FeOx≥95.0% are prepared in a weight percentage ratio of 60:10:30. The particle size of the powdered dephosphorization agent is controlled to be 3-5 mm.

[0014] Furthermore, in the above-mentioned method for deep dephosphorization of chromium-nickel pig iron melt in electric furnace, the composition of desiliconized slag is controlled as follows: TFe: 10-15%, CaO: 45-50%, SiO 2 : 18~20%, MgO: 5~7%, Cr 2 O 3 :8~15%.

[0015] Furthermore, in the above-mentioned method for deep dephosphorization of chromium-nickel pig iron melt smelted in an electric furnace, the composition of the dephosphorization slag is controlled to be: TFe: 18-25%, CaO: 35-45%, SiO 2 : 5~8%, MgO: 6~9%, CaF 2 :8~10%.

[0016] Furthermore, in the above-mentioned method for deep dephosphorization of chromium-nickel pig iron melt smelted in an electric furnace, in the desiliconization and dechromization operation of step 2, the oxygen pressure is controlled to be 1.0 Mp, and the angle between the furnace door oxygen lance and the molten steel surface is controlled to be 25-30°.

[0017] Furthermore, in the above-mentioned method for deep dephosphorization of chromium-nickel pig iron melt smelted in an electric furnace, in the deep dephosphorization operation in the electric furnace in step 4, the oxygen pressure is controlled to be 1.0 MPa, and the angle between the furnace door oxygen lance and the molten steel surface is controlled to be 30-40°.

[0018] Furthermore, in the above-mentioned method for deep dephosphorization of chromium-nickel pig iron molten metal in electric furnace smelting, the composition of the chromium-nickel pig iron is: C≤3.0%, Si≤2.5%, P≤0.050%, Cr≤4.0%, Ni: 7-15%, and the rest is iron and residual elements.

[0019] The method for deep dephosphorization of chromium-nickel pig iron melt smelted in an electric furnace of the present invention has the following advantages and beneficial effects: the present invention solves the technical problem of high cost caused by the need to use dephosphorized molten iron + pure nickel for stainless steel smelting due to the difficulty in electric furnace dephosphorization of chromium-nickel pig iron melt, and achieves the purpose of using cheap chromium-nickel pig iron as a raw material to prepare a low-phosphorus high-nickel stainless steel mother liquor through deep dephosphorization in an electric furnace, and using the low-phosphorus high-nickel stainless steel mother liquor to add high-carbon ferrochrome to produce a low-phosphorus special stainless steel variety. The smelting of low-phosphorus stainless steel no longer uses blast furnace dephosphorized molten iron, and the blast furnace molten iron production process is cancelled, thereby simplifying the production process and reducing carbon emissions. In addition, since there is no need to use expensive pure nickel, the smelting cost of low-phosphorus stainless steel is reduced, and the method has good promotion value and economic benefits. DETAILED DESCRIPTION

[0020] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the specific embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0021] The invention aims to solve the technical problem of high cost caused by the need to use dephosphorized molten iron + pure nickel in stainless steel smelting due to the difficulty in dephosphorizing chromium-nickel pig iron melt in an electric furnace, and develops a method for deep dephosphorization of chromium-nickel pig iron melt in an electric furnace. The electric furnace uses chromium-nickel pig iron as a raw material to produce a low-phosphorus high-nickel stainless steel mother liquor with P≤0.004%. The basic process is: the electric furnace uses chromium-nickel pig iron as a raw material, melts to form a chromium-nickel pig iron pre-melt, first desiliconizes and dechromizes, and after desiliconization and dechromization are completed, the desiliconized slag is poured out from the furnace door, and then deep dephosphorization is started to produce a low-phosphorus high-nickel stainless steel mother liquor.

[0022] Specifically, the method for deep dephosphorization of chromium-nickel pig iron melt smelted in an electric furnace of the present invention comprises the following steps:

[0023] (1) An electric furnace is charged with chromium-nickel pig iron, and the chromium-nickel pig iron is melted to form a chromium-nickel pig iron pre-melt, wherein the composition of the chromium-nickel pig iron is: C≤3.0%, Si≤2.5%, P≤0.050%, Cr≤4.0%, Ni: 7-15%, and the rest is iron and residual elements.

[0024] (2) After the electric furnace is smelted, desiliconization and dechromization are first performed, and the desiliconization and dechromization operation is performed by a solid-gas oxidation desiliconization and dephosphorization method. In this process, a solid dephosphorization agent is added from the high-level material bin of the electric furnace in batches for multiple times. The total amount of solid dephosphorization agent added per ton of steel is controlled to be 20-25 kg. The solid dephosphorization agent is prepared from converter dust, sintered ore and light-burned magnesium powder in a weight percentage ratio of 70:20:10. The composition of the solid dephosphorization agent is: FeOx: 56-70%, CaO: 10-18%, MgO: 3-8%, SiO 2 : 1.5~3%; oxygen is supplied by furnace door oxygen lance, oxygen pressure is controlled at 1.0Mpa, oxygen flow rate per ton of steel is controlled at 0.24~0.32Nm 3 / min, the angle between the oxygen lance at the furnace door and the molten steel surface is controlled at 25-30°; lime is added in batches during the process, and the total amount of lime added is controlled to be 15-20 kg per ton of steel, and the desiliconized slag with a basicity of 1.8-2.5 is produced. The composition of the desiliconized slag is controlled to be: TFe: 10-15%, CaO: 45-50%, SiO 2 : 18~20%, MgO: 5~7%, Cr 2 O 3: 8-15%, during the smelting process, the electric furnace continuously supplies electrochemical slag to control the temperature of the molten steel in the electric furnace at 1420-1480℃.

[0025] (3) When Si≤0.02% and Cr≤0.80% in the molten steel, stop desiliconization and dechromization, and carry out the electric furnace slag removal operation to remove most of the desiliconization slag, and the proportion of the slag removal to the total slag volume is ≥70%.

[0026] (4) After the slagging is completed, the deep dephosphorization operation of the electric furnace is carried out. Solid dephosphorization agent is added in batches from the high-level silo of the electric furnace for multiple times. The total amount of solid dephosphorization agent added per ton of steel is controlled to be 15-18 kg; the oxygen lance at the furnace door continues to supply oxygen, the oxygen pressure is controlled to be 1.0 MPa, and the oxygen supply flow rate per ton of steel is controlled to be 0.30-0.38 Nm 3 / min, the angle between the oxygen lance at the furnace door and the molten steel surface is controlled at 30-40° to enhance the stirring effect of the electric furnace. At the same time, the carbon powder gun of the electric furnace sprays powdered dephosphorization agent, which is composed of lime powder with CaO ≥ 90.0%, CaF 2 ≥88.0% of fluorite powder and FeOx≥95.0% of iron oxide powder are prepared in a weight percentage ratio of 60:10:30. The particle size of the powdered dephosphorization agent is controlled to be 3-5mm. The carrier gas for spraying the powdered dephosphorization agent is nitrogen, and the nitrogen pressure is controlled to be 1.0MPa. During the dephosphorization process, lime is added in batches from a high position, and the total amount of lime added is controlled to be 15-18kg per ton of steel. The dephosphorization slag with an alkalinity of 5-8 is used for deep dephosphorization. The composition of the dephosphorization slag is controlled to be: TFe: 18-25%, CaO: 35-45%, SiO 2 : 5~8%, MgO: 6~9%, CaF 2 : 8-10%, during the dephosphorization process, the electric furnace continuously supplies electrochemical slag to control the molten steel temperature at 1500-1550℃.

[0027] (5) When P in molten steel is less than or equal to 0.004%, dephosphorization is terminated, oxygen lance at furnace door stops blowing oxygen, and nitrogen is blown for strong stirring. The nitrogen supply flow rate per ton of steel is controlled at 0.35-0.45 Nm 3 / min, stir for 3 to 5 minutes to promote uniform temperature and composition of the molten steel, continue to supply power to the electric furnace to raise the temperature to above 1630℃, remove the dephosphorization slag, the slag removal amount accounts for ≥80% of the total slag, and produce low-phosphorus high-nickel stainless steel mother liquor, which can be subsequently sent to the AOD furnace for refining of low-phosphorus special stainless steel with P≤0.015%.

[0028] The method for deep dephosphorization of chromium-nickel pig iron melt from electric furnace smelting of the present invention is described in detail below in conjunction with specific embodiments of the present invention.

[0029] Example 1

[0030] Example 1 of the present invention is used to melt chromium-nickel pig iron in a 160-ton electric furnace and perform deep dephosphorization in the electric furnace to produce a low-phosphorus high-nickel stainless steel mother liquor for AOD production of low-phosphorus stainless steel varieties. The specific implementation process is as follows:

[0031] (1) 165 tons of chrome-nickel pig iron is loaded into an electric furnace, and the composition of the chrome-nickel pig iron is: C: 2.5%, Si: 1.5%, P: 0.050%, Ni: 15%, Cr: 2.5%, and the rest is iron and residual elements. The electric furnace is powered to melt the chrome-nickel pig iron into a chrome-nickel pig iron pre-melt. After melting, desiliconization and dechromization are first performed, and the desiliconization and dechromization operations are performed by a solid-gas oxidation desiliconization and dephosphorization method. In this process, a solid dephosphorization agent is added from a high-level silo of the electric furnace in batches for multiple times. The total amount of solid dephosphorization agent added is 3.3 tons. The solid dephosphorization agent is prepared from converter dust, sintered ore and light-burned magnesium powder in a weight percentage of 70:20:10. The composition of the solid dephosphorization agent is: FeOx: 70%, CaO: 18%, MgO: 5%, SiO 2 : 2%; oxygen is supplied by furnace door oxygen gun, oxygen pressure is 1.0Mpa, oxygen flow rate is 45Nm 3 / min, the angle between the oxygen lance at the furnace door and the molten steel surface is 25°; lime is added in batches during the process, and the total amount of lime added is controlled to be 3 tons, and the desiliconized slag with a basicity of 1.8-2.5 is produced. The desiliconized slag composition is: TFe: 12%, CaO: 48%, SiO 2 :19%、MgO:6%、Cr 2 O 3 : 13%, during the smelting process, the electric furnace continuously supplies electrochemical slag to control the temperature of the molten steel in the electric furnace at 1420 ~ 1450 ℃.

[0032] (2) When Si≤0.02% and Cr≤0.80% in molten steel, stop desiliconization and dechromization, and carry out electric furnace slag removal operation to remove more than 70% of the desiliconization slag.

[0033] (3) After the slagging is completed, the deep dephosphorization operation of the electric furnace is carried out. Solid dephosphorization agent is added in batches from the high-level silo of the electric furnace for multiple times. The total amount of solid dephosphorization agent added is controlled to be 2.9 tons; the oxygen lance at the furnace door continues to supply oxygen, the oxygen pressure is 1.0Mpa, and the oxygen flow rate is 60Nm 3 / min, the angle between the oxygen lance at the furnace door and the molten steel surface is 35°, the stirring effect of the electric furnace is enhanced, and at the same time, the carbon powder gun of the electric furnace sprays powdered dephosphorization agent, which is composed of lime powder with CaO ≥ 90.0%, CaF 2Fluorite powder ≥88.0% and iron oxide powder FeOx ≥95.0% are prepared in a weight percentage ratio of 60:10:30. The particle size of the powdered dephosphorization agent is controlled to be 3-5 mm. The carrier gas for spraying the powdered dephosphorization agent is nitrogen, and the nitrogen pressure is 1.0 MPa. During the dephosphorization process, lime is added in batches from a high position, and the total amount of lime added is 2.9 tons. The dephosphorization slag with an alkalinity of 6.7 is used for deep dephosphorization. The composition of the dephosphorization slag is: TFe: 20%, CaO: 40%, SiO 2 :6%、MgO:8%、CaF 2 : 9%, during the dephosphorization process, the electric furnace continuously supplies electrolytic slag to control the molten steel temperature at 1530℃.

[0034] (4) When P in molten steel is less than or equal to 0.004%, dephosphorization is terminated, oxygen lance at furnace door stops blowing oxygen, and nitrogen is blown for strong stirring. The nitrogen supply flow rate is 65 Nm 3 / min, stirring for 3min to promote uniform temperature and composition of the molten steel, the electric furnace continues to supply power to raise the temperature to above 1650℃, more than 80% of the dephosphorization slag is removed, and low-phosphorus and high-nickel stainless steel mother liquor is produced.

[0035] By using Example 1, 160 tons of low-phosphorus, high-nickel stainless steel mother liquor were finally prepared, and the steel composition was: C: 1.0%, Si: 0.01%, P: 0.004%, Ni: 15%, Cr: 0.40%. The low-phosphorus, high-nickel stainless steel mother liquor can be subsequently sent to an AOD furnace for refining of a special type of low-phosphorus stainless steel with P ≤ 0.015%.

[0036] In summary, the method for deep dephosphorization of chromium-nickel pig iron melt in an electric furnace of the present invention uses chromium-nickel pig iron as a raw material for electric furnace deep dephosphorization, adds a solid dephosphorizing agent into the electric furnace, sprays a powdered dephosphorizing agent, and blows oxygen into the oxygen gun for coordinated dephosphorization to produce a low-phosphorus high-nickel stainless steel mother liquor, and the electric furnace endpoint phosphorus content of the low-phosphorus high-nickel stainless steel mother liquor reaches the target of P≤0.004%, and can be directly used as a stainless steel mother liquor in an AOD furnace for refining low-phosphorus special stainless steel with P≤0.015%.

[0037] Compared with the prior art, the method for deep dephosphorization of chromium-nickel pig iron melt smelted in an electric furnace of the present invention has the following advantages and beneficial effects: the present invention solves the technical problem of high cost caused by the need to use dephosphorized molten iron + pure nickel for stainless steel smelting due to the difficulty in electric furnace dephosphorization of chromium-nickel pig iron melt, and achieves the purpose of using cheap chromium-nickel pig iron as a raw material to prepare a low-phosphorus high-nickel stainless steel mother liquor through deep dephosphorization in an electric furnace, and using the low-phosphorus high-nickel stainless steel mother liquor to add high-carbon ferrochrome to produce a low-phosphorus special stainless steel variety. The smelting of low-phosphorus stainless steel no longer uses blast furnace dephosphorized molten iron, and the blast furnace molten iron production process is cancelled, thereby simplifying the production process and reducing carbon emissions. In addition, since there is no need to use expensive pure nickel, the smelting cost of low-phosphorus stainless steel is reduced, and the method has good promotion value and economic benefits.

[0038] It should be noted that, in this article, the term "comprise" or any other variation thereof is intended to cover non-exclusive inclusion, so that an article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such article or device.

[0039] It should also be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the present invention.

Claims

1. A method for deep dephosphorization of chromium-nickel pig iron melt from electric furnace smelting, characterized in that: The steps include: Step 1: Load chromium-nickel pig iron into an electric furnace and melt the chromium-nickel pig iron to form a chromium-nickel pig iron pre-melt; Step 2: After the electric furnace is melted, desiliconization and dechromization operations are carried out. In this process, solid dephosphorization agent is added in batches from the high-level silo of the electric furnace for multiple times. The total amount of solid dephosphorization agent added per ton of steel is controlled to be 20-25 kg. Oxygen is supplied by the furnace door oxygen lance, and the oxygen supply flow rate per ton of steel is controlled to be 0.24-0.32 Nm 3 / min; lime is added in batches during the process, and the total amount of lime added is controlled to be 15-20kg per ton of steel, and desiliconized slag with a basicity of 1.8-2.5 is produced. During the smelting process, the electric furnace continuously supplies electrified slag to control the temperature of the molten steel in the electric furnace at 1420-1480℃; Step 3: When Si≤0.02% and Cr≤0.80% in the molten steel, stop desiliconization and dechromization, perform electric furnace slag removal, and remove ≥70% of the desiliconization slag; Step 4: After slagging, deep dephosphorization is carried out in the electric furnace. Solid dephosphorization agent is added from the high-level silo in batches for multiple times. The total amount of solid dephosphorization agent added per ton of steel is controlled to be 15-18 kg. The oxygen lance at the furnace door continues to supply oxygen, and the oxygen flow rate per ton of steel is controlled to be 0.30-0.38 Nm 3 / min, and at the same time, the electric furnace carbon powder gun sprays powdered dephosphorization agent, and the carrier gas for spraying the powdered dephosphorization agent is nitrogen, and the nitrogen pressure is controlled to be 1.0MPa; during the dephosphorization process, lime is added in batches from a high position, and the total amount of lime added is controlled to be 15-18kg per ton of steel, and dephosphorization slag with a basicity of 5-8 is used for deep dephosphorization. During the dephosphorization process, the electric furnace continuously supplies electrified slag to control the molten steel temperature at 1500-1550℃; Step 5: When P in the molten steel is less than or equal to 0.004%, dephosphorization is terminated, oxygen lance at the furnace door stops blowing oxygen, and nitrogen is blown for strong stirring. The nitrogen supply flow rate per ton of steel is controlled to be 0.35-0.45Nm 3 / min, stir for 3 to 5 minutes, continue to supply power to the electric furnace to raise the temperature to above 1630℃, remove ≥80% of the dephosphorization slag, and produce low-phosphorus and high-nickel stainless steel mother liquor.

2. The method for deep dephosphorization of chromium-nickel pig iron melt from electric furnace smelting as claimed in claim 1, characterized in that: The solid dephosphorization agent is prepared from converter dust, sintered ore and light-burned magnesium powder in a weight percentage ratio of 70:20:

10. The composition of the solid dephosphorization agent is controlled as follows: FeOx: 56-70%, CaO: 10-18%, MgO: 3-8%, SiO2: 1.5-3%.

3. The method for deep dephosphorization of chromium-nickel pig iron melt from electric furnace smelting as claimed in claim 2, characterized in that: The powdery dephosphorization agent is prepared from lime powder with CaO≥90.0%, fluorite powder with CaF2≥88.0%, and iron oxide powder with FeOx≥95.0% in a weight percentage ratio of 60:10:30, and the particle size of the powdery dephosphorization agent is controlled to be 3-5 mm.

4. The method for deep dephosphorization of chromium-nickel pig iron melt from electric furnace smelting as claimed in claim 3, characterized in that: The composition of the desiliconized slag is controlled as follows: TFe: 10-15%, CaO: 45-50%, SiO2: 18-20%, MgO: 5-7%, Cr2O3: 8-15%.

5. The method for deep dephosphorization of chromium-nickel pig iron melt from electric furnace smelting as claimed in claim 4, characterized in that: The composition of the dephosphorization slag is controlled as follows: TFe: 18-25%, CaO: 35-45%, SiO2: 5-8%, MgO: 6-9%, CaF2: 8-10%.

6. The method for deep dephosphorization of chromium-nickel pig iron melt from electric furnace smelting as claimed in claim 1, characterized in that: In the desiliconization and dechromization operation of step 2, the oxygen pressure is controlled to be 1.0 Mp, and the angle between the furnace door oxygen lance and the molten steel surface is controlled to be 25-30°.

7. The method for deep dephosphorization of chromium-nickel pig iron melt from electric furnace smelting as claimed in claim 1, characterized in that: In the electric furnace deep dephosphorization operation of step 4, the oxygen pressure is controlled to be 1.0 MPa, and the angle between the furnace door oxygen lance and the molten steel surface is controlled to be 30-40°.

8. The method for deep dephosphorization of chromium-nickel pig iron melt from electric furnace smelting according to any one of claims 1 to 7, characterized in that: The composition of chromium-nickel pig iron is: C≤3.0%, Si≤2.5%, P≤0.050%, Cr≤4.0%, Ni: 7~15%, and the rest is iron and residual elements.

Citation Information

Patent Citations

  • Process for manufacturing stainless steel by using high-phosphorus nickel-chromium pig iron

    CN101705332A

  • Dephosphorization method of high-phosphorous chromium-nickel pig iron

    CN102312033A

  • Oxidizing dephosphorization method for high-silicon high-phosphorus chromium-nickel-containing molten iron

    CN104673970A

  • Smelting method of 310S heat-resistant stainless steel

    CN116926408A

  • Process method for smelting duplex stainless steel at low cost

    CN117344086A