Method for improving performance of high-strength steel
By adjusting the annealing process parameters of high-strength steel and monitoring the optical elongation, the problem of yield strength fluctuations in different batches of high-strength steel is solved, the stability of temperature and mechanical properties is achieved, and the production reliability and accuracy are significantly improved.
Patent Information
- Application Number
- CN202411118426.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-15
AI Technical Summary
During different batches of high-strength steel, the yield strength fluctuates greatly due to the difference in annealing process, which affects the assembly accuracy of parts and stamping production rhythm. It is difficult for the existing technology to achieve accurate temperature measurement, resulting in unstable performance.
By obtaining the indirect temperature and theoretical temperature of the heat-supporting section of the reference strip, adjust the annealing process parameters such as gas flow, atmosphere temperature in the furnace and heat-supporting time to maintain the temperature stability of different furnace areas, and monitor the light-integrated elongation and rolling Control force ensures consistency of temperature and mechanical properties.
It effectively reduces the yield strength fluctuations between different batches of high-strength steel, improves performance stability, significantly improves the yield strength differences between batches, and improves the reliability and accuracy of production.
Smart Images

Figure CN119061241A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of automobile steel and engineering structure steel, and in particular to a method for improving the performance of high-strength steel. Background Art
[0002] High-strength steel represented by dual-phase steel (DP steel) has the advantages of good comprehensive formability, mature production process and low cost, and has been widely used in body-in-white. In the annealing production process of high-strength steel, since the production is continuous, it is difficult to directly measure the strip temperature by thermocouple. Usually, a radiation pyrometer is used to indirectly measure the strip surface. However, the strip temperature measured by the pyrometer is different from the indirect strip temperature, which makes it difficult to accurately measure the high-strength steel strip temperature, thus causing performance fluctuations.
[0003] In the indirect production process, it is often the case that high-strength steel of the same brand and specification has no obvious difference in the annealing process when produced in different batches, but the measured yield strength fluctuates significantly, which will have an adverse impact on the use of downstream customers. Under the same forming conditions, due to the higher yield strength of high-strength steel, it is more likely to produce springback than traditional soft steel, which has an adverse effect on the assembly accuracy of parts and the rhythm of stamping production. Therefore, the performance stability of high-strength steel has become one of the focuses of attention in the automotive industry. Although the springback phenomenon can be effectively improved by die compensation technology at present, when the yield strength of high-strength steel produced in different batches fluctuates greatly, the stamping die needs to be adjusted frequently; if the yield fluctuation is too large, even adjusting the die cannot compensate for the springback. Therefore, there is an urgent need for a method to effectively improve the stability of the yield strength of high-strength steel between different batches. Summary of the invention
[0004] The present application provides a method for improving the performance of high-strength steel to solve the following technical problem: how to improve the yield strength difference of different batches of high-strength steel.
[0005] In a first aspect, the present application provides a method for improving the performance of high-strength steel, the method comprising:
[0006] Obtain the indirect temperature of the first soaking section in the furnace and the theoretical temperature of the first soaking section in the furnace of the reference strip;
[0007] Annealing the current steel strip, and obtaining the indirect temperature of the second soaking section in the furnace and the theoretical temperature of the second soaking section in the furnace at the corresponding moments of the current steel strip and the reference steel strip;
[0008] Determine whether a first difference between the theoretical temperature of the soaking section in the first furnace and the theoretical temperature of the soaking section in the second furnace is within a first set interval, wherein a second difference between the indirect temperature of the soaking section in the first furnace and the indirect temperature of the soaking section in the second furnace is within a second set interval;
[0009] If not, the process parameters of the annealing and soaking section of the current steel strip are adjusted so that the first difference is within the first set range, wherein the process parameters include: gas flow rate.
[0010] Optionally, the first setting interval is -10°C to 10°C.
[0011] Optionally, the second setting interval is -10°C to 10°C.
[0012] Optionally, the process parameters also include: furnace atmosphere temperature, soaking temperature, soaking time and strip running speed.
[0013] Optionally, the method further includes:
[0014] Acquire the skin pass elongation of the reference steel strip and a first rolling force corresponding to the skin pass elongation;
[0015] Perform skin-pass on the current steel strip to obtain a second rolling force of the current steel strip corresponding to the skin-pass elongation;
[0016] Based on the first rolling force, determining whether the fluctuation amplitude of the second rolling force is within a third set range;
[0017] If not, the current finishing elongation is adjusted until the fluctuation amplitude is within the third setting range.
[0018] Optionally, the third setting interval is ≤10%.
[0019] Optionally, the tensile strength of the high-strength steel is ≥780Mpa.
[0020] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0021] The method for improving the performance of high-strength steel provided in an embodiment of the present application includes: obtaining the indirect temperature of the first in-furnace soaking section and the theoretical temperature of the first in-furnace soaking section of a reference strip; annealing the current strip to obtain the indirect temperature of the second in-furnace soaking section and the theoretical temperature of the second in-furnace soaking section at corresponding moments of the current strip and the reference strip; judging whether a first difference between the theoretical temperature of the first in-furnace soaking section and the theoretical temperature of the second in-furnace soaking section is within a first set interval, wherein a second difference between the indirect temperature of the first in-furnace soaking section and the indirect temperature of the second in-furnace soaking section is within a second set interval; if not, adjusting the process parameters of the annealing soaking section of the current strip so that the first difference is within the first set interval, wherein the process parameters include: gas flow rate. During the continuous annealing production process of high-strength steel strip, the indirect temperature of the first soaking section in the furnace and the theoretical temperature of the first soaking section in the furnace are obtained for the reference strip. The indirect temperature of the second soaking section in the furnace and the theoretical temperature of the second soaking section in the furnace for the subsequent high-strength steel strip of the same brand, specification and process are used as judgment criteria. The theoretical temperature of the soaking sections in different furnace zones is kept at a fixed value, thereby ensuring the temperature stability of the high-strength steel strip in different areas of the furnace, thereby improving the yield strength difference of different batches of high-strength steel. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0023] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0024] Figure 1 A schematic flow chart of a method for improving the performance of high-strength steel according to some embodiments of the present application;
[0025] Figure 2 This is a bar chart comparing the yield strength fluctuations between batches of hot-dip galvanized DP980 before and after improvement. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0027] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0028] In this application, the terms "include", "comprising", etc. mean "including but not limited to". In this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such indirect relationship or order between these entities or operations.
[0029] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0030] In the annealing process of high-strength steel, since the production is continuous, it is difficult to directly measure the temperature of the strip by thermocouple. Usually, a radiation pyrometer is used to indirectly measure the surface of the strip. An important disadvantage of the radiation pyrometer is that infrared radiation strongly depends on the surface emissivity of the steel plate, and the accurate measurement of the surface emissivity of the steel plate is an industry-wide difficulty. Therefore, there is a difference between the strip temperature measured by the pyrometer and the indirect temperature of the strip. However, this difference will change with the change of the surface state of the strip, which will cause large fluctuations in the performance of the strip produced in different batches. For example, the surface state of the high-strength steel chilled coil is affected by the hot rolling process, pickling process, cold rolling process, furnace cleaning process and even the annealing furnace atmosphere. Changes in process parameters in any link may cause changes in the surface emissivity of the steel plate, thereby affecting the temperature measurement accuracy and ultimately affecting the mechanical properties of the finished product. In addition, changes in the state of the pyrometer itself will also affect the accuracy of temperature measurement, and the measurement angle of the pyrometer and the cleanliness of the lens will affect the accuracy of temperature measurement. Since the annealing furnace is a black box, it is impossible to calibrate the angle or clean the lens during normal production of steel plates; once an abnormality occurs during pyrometer detection, it is often not discovered in time. Therefore, changes in the surface state of the steel plate and the state of the pyrometer itself will affect the accurate measurement of the temperature of the high-strength steel strip, resulting in performance fluctuations.
[0031] Therefore, the present application provides a method for improving the performance of high-strength steel. Figure 1 For a flow chart of a method for improving the performance of high-strength steel according to some embodiments of the present application, see Figure 1 , the method comprising:
[0032] S1. Obtaining the indirect temperature of the first soaking section in the furnace and the theoretical temperature of the first soaking section in the furnace for the reference steel strip;
[0033] Annealing the current steel strip, and obtaining the indirect temperature of the second soaking section in the furnace and the theoretical temperature of the second soaking section in the furnace at the corresponding moments of the current steel strip and the reference steel strip;
[0034] Determine whether a first difference between the theoretical temperature of the soaking section in the first furnace and the theoretical temperature of the soaking section in the second furnace is within a first set interval, wherein a second difference between the indirect temperature of the soaking section in the first furnace and the indirect temperature of the soaking section in the second furnace is within a second set interval;
[0035] If not, the process parameters of the annealing and soaking section of the current steel strip are adjusted so that the first difference is within the first set range, wherein the process parameters include: gas flow rate.
[0036] In some embodiments, the first setting interval is -10°C to 10°C.
[0037] In some embodiments, the second setting interval is -10°C to 10°C.
[0038] In some embodiments, the process parameters further include: furnace atmosphere temperature, soaking temperature, soaking time and strip running speed.
[0039] In the embodiment of the present application, a representative high-strength steel (dual-phase steel) is used. Since the emissivity of the dual-phase steel surface is affected by various factors such as the hot rolling process, the pickling process, the cold rolling process, the furnace cleaning process, and the annealing furnace atmosphere, the temperature measured by the pyrometer (the indirect temperature of the soaking section in the furnace) T D The indirect temperature of high-strength steel is more or less different; and the same grade and specification of high-strength steel produced in different batches will also fluctuate due to slight differences in the whole process, resulting in fluctuations in yield strength and other performance indicators. In order to avoid significant fluctuations in the mechanical properties of high-strength steel produced in different batches, in addition to monitoring the displayed temperature of the pyrometer, it is also necessary to calculate the strip temperature of the furnace area (theoretical temperature of the soaking section in the furnace) T C Monitor. C The calculation model is provided by the secondary computer of the production line, which can be controlled by gas flow, furnace atmosphere temperature, soaking temperature, soaking time and strip running speed. Because the strip absorbs heat from the furnace through radiation, heat conduction and other means in the annealing furnace, in theory, the T of strips of the same grade, specification and process produced in different batches is the same. C If the surface conditions of the two batches of strip steel change significantly (i.e. the surface emissivity changes significantly), the T displayed in the pyrometer control mode will be D Same, but with steel T C At this time, the pyrometer control mode should be switched to the calculated temperature control mode, that is, the T of different furnace zones should be kept constant. C At a certain fixed value, the temperature stability of the strip in different areas of the furnace is ensured. For example, for a certain grade of strip steel of a certain specification, a reference strip steel with normal performance is selected, and the temperature value T of the reference strip steel is calculated. C ; For subsequent production of high-strength steel of the same grade and specification, it is necessary to control T D The difference between the value and the reference strip steel is not obvious (≤±10℃), T C The fluctuation T of the value and the reference strip C The fluctuation of the value is controlled within ±10℃.
[0040] In some embodiments, the method further comprises:
[0041] S2. Obtaining the skin pass elongation of the reference steel strip and a first rolling force corresponding to the skin pass elongation;
[0042] Perform skin-pass on the current steel strip to obtain a second rolling force of the current steel strip corresponding to the skin-pass elongation;
[0043] Based on the first rolling force, determining whether the fluctuation amplitude of the second rolling force is within a third set range;
[0044] If not, the current finishing elongation is adjusted until the fluctuation amplitude is within the third setting range.
[0045] In some embodiments, the third setting interval is ≤10%.
[0046] In some embodiments, the tensile strength of the high-strength steel is ≥780 MPa.
[0047] In the embodiment of the present application, in order to further improve the performance stability of different batches of high-strength steel, the elongation and rolling force of the skin-pass mill should also be monitored at the same time. Usually, the skin-pass mill is controlled in a constant elongation mode, but when the temperature of a certain high-strength steel indirect strip produced in different batches is significantly different, the constant elongation mode will aggravate the fluctuation of yield strength, so the skin-pass rolling force should also be monitored during production. Exemplarily, for a certain specification of strip steel of a certain grade, a reference strip steel with normal performance is selected, and the skin-pass rolling force of the reference strip steel corresponding to the skin-pass elongation is recorded; for the subsequent production of high-strength steel of the same grade and specification, under the condition of using the same skin-pass elongation, the skin-pass rolling force fluctuation needs to be controlled within 10%, and the current skin-pass elongation can be adjusted manually until the fluctuation amplitude is within the third set interval.
[0048] The above method for improving the performance of high-strength steel is applicable to high-strength steel of all composition systems and strength levels, especially high-strength steel with a tensile strength of ≥780Mpa. For example, after adopting the above method for improving the performance of high-strength steel, the yield strength fluctuation between batches of hot-dip galvanized DP980 is reduced from about 130MPa to about 80MPa, and the improvement effect is significant.
[0049] Exemplarily, a full process for preparing dual-phase steel includes: smelting, continuous casting, heating, hot rolling, pickling, cold rolling, annealing, galvanizing and skin-passing. Among them, the heating temperature is 1150-1250℃, the hot rolling final rolling temperature is 900℃, the coiling temperature is 250℃, and the hot-rolled plate is pickled, annealed and galvanized. The slab heating temperature is between 1150-1250℃ for homogenization of the structure and solid solution of micro-alloying elements. Too high a temperature may cause abnormal growth of grains, and too low a temperature may cause uneven composition and insufficient solid solution of micro-alloying elements. The final rolling temperature is set at 900℃ mainly to ensure a good hot rolling structure. If the final rolling temperature is too high, the grains may become coarse, and if the final rolling temperature is too low, mixed crystals may appear. The coiling temperature is set at 250℃ to obtain a full martensitic structure. A coiling temperature below 200℃ will cause coiling difficulties, and a coiling temperature that is too high will make it difficult to obtain full martensite.
[0050] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0051] The present application provides a method for improving the performance of high-strength steel, the method comprising:
[0052] S11, obtaining the indirect temperature of the first soaking section in the furnace and the theoretical temperature of the first soaking section in the furnace of the reference steel strip;
[0053] Annealing the current steel strip, and obtaining the indirect temperature of the second soaking section in the furnace and the theoretical temperature of the second soaking section in the furnace at the corresponding moments of the current steel strip and the reference steel strip;
[0054] Determine whether a first difference between the theoretical temperature of the soaking section in the first furnace and the theoretical temperature of the soaking section in the second furnace is within a first set interval, wherein a second difference between the indirect temperature of the soaking section in the first furnace and the indirect temperature of the soaking section in the second furnace is within a second set interval;
[0055] If not, the process parameters of the annealing and soaking section of the current steel strip are adjusted so that the first difference is within the first set range, wherein the process parameters include: gas flow rate.
[0056] S21, obtaining the skin pass elongation of the reference steel strip and a first rolling force corresponding to the skin pass elongation;
[0057] Perform skin-pass on the current steel strip to obtain a second rolling force of the current steel strip corresponding to the skin-pass elongation;
[0058] Based on the first rolling force, determining whether the fluctuation amplitude of the second rolling force is within a third set range;
[0059] If not, the current finishing elongation is adjusted until the fluctuation amplitude is within the third setting range.
[0060] In the embodiment of the present application, the indirect temperature T D The theoretical temperature (calculated temperature) of the soaking section in the furnace is measured by a pyrometer. C The second difference between the indirect temperature of the soaking section in the first furnace and the indirect temperature of the soaking section in the second furnace is measured by the calculation model of the secondary computer of the continuous hot-dip galvanizing zinc production line, and is regulated by the gas flow, the atmosphere temperature in the furnace, the soaking temperature, the soaking time, and the running speed of the strip steel. Specifically, please refer to the chemical composition (wt%) of the high-strength steel shown in Table 1, and the annealing process parameters of the high-strength steel shown in Table 2; please refer to the control mode results in the method for improving the performance of high-strength steel shown in Table 3, and please refer to the mechanical properties of the high-strength steel shown in Table 4.
[0061] Table 1 Chemical composition of high-strength steel (wt%), the rest is Fe and unavoidable impurities
[0062] Steel Type C Si Mn Cr Al P S Nb Ti DP780 0.10 0.3 2.0 0.15 0.03 0.010 0.002 0.015 0.012 DP980 0.11 0.35 2.3 0.45 0.04 0.011 0.003 0.02 0.018
[0063] Table 2 Annealing process parameters of high strength steel
[0064]
[0065] Table 3 Control mode results in the method of improving the properties of high-strength steel
[0066]
[0067]
[0068] Table 4 Mechanical properties of high strength steel
[0069]
[0070] In summary, Comparative Example 1 shows the yield strength fluctuation of two batches produced under the conventional pyrometer + skin-finishing elongation control mode. The total number of rolls in the two batches is 90 rolls, and the pyrometer measurement value T of the average temperature of the two batches is D The difference is not big, but the calculated temperature T C There are obvious differences, and the T C The fluctuation value is above 20℃, indicating that the indirect temperature of the strip steel in different coils will be significantly different; in addition, the skin-pass rolling force fluctuation of each batch is also above 10%, and the yield strength fluctuation between the final batches is as high as 121MPa. Comparative Example 2 is the pyrometer + skin-pass elongation / rolling force control mode, TD and T C The fluctuation of is similar to that of comparative example 1, but because the skin-pass elongation and rolling force are monitored at the same time, the rolling force fluctuation of each batch is reduced to less than 10%, resulting in an improvement in the yield strength fluctuation between batches, which is reduced to 102MPa. Example 1 is a pyrometer / calculated temperature + skin-pass elongation / rolling force control mode. Since T is monitored at the same time, D and T C , resulting in each batch T D and T C The fluctuation was significantly improved, and coupled with the improvement effect of simultaneous monitoring of the skin-clearing elongation and rolling force, the yield strength between batches was further reduced to 75MPa, and the improvement effect was more obvious.
[0071] Comparative Example 3 shows the yield strength fluctuation under the conventional pyrometer + skin-finishing elongation control mode, T D and T C The fluctuation of rolling force is similar to that of comparative example 1, with a yield fluctuation of 134 MPa between batches. Comparative example 4 shows the improvement after using pyrometer + skin-pass elongation / rolling force, with the yield fluctuation between batches reduced to 112 MPa. Example 2 shows the situation after using pyrometer / calculated temperature + skin-pass elongation / rolling force control mode, with the yield fluctuation between batches further reduced to 79 MPa, with a significant improvement effect. Figure 2 This is a bar chart comparing the yield strength fluctuations between batches of hot-dip galvanized DP980 before and after improvement; please refer to Figure 2 , indicating that the hot-dip galvanized DP980 adopts the method for improving the performance of high-strength steel provided in the embodiment of the present application, which significantly reduces the yield strength fluctuation between batches of hot-dip galvanized DP980.
[0072] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for improving the performance of high-strength steel, characterized in that: The method comprises: Obtain the indirect temperature of the first soaking section in the furnace and the theoretical temperature of the first soaking section in the furnace of the reference steel strip; Annealing the current steel strip, and obtaining the indirect temperature of the second soaking section in the furnace and the theoretical temperature of the second soaking section in the furnace at the corresponding moments of the current steel strip and the reference steel strip; Determine whether a first difference between the theoretical temperature of the soaking section in the first furnace and the theoretical temperature of the soaking section in the second furnace is within a first set interval, wherein a second difference between the indirect temperature of the soaking section in the first furnace and the indirect temperature of the soaking section in the second furnace is within a second set interval; If not, the process parameters of the annealing and soaking section of the current steel strip are adjusted so that the first difference is within the first set range, wherein the process parameters include: gas flow rate.
2. The method according to claim 1, characterized in that: The first setting interval is -10°C to 10°C.
3. The method according to claim 1, characterized in that The second setting range is -10°C to 10°C.
4. The method according to claim 1, characterized in that: The process parameters also include: furnace atmosphere temperature, soaking temperature, soaking time and strip running speed.
5. The method according to claim 1, characterized in that The method further comprises: Acquire the skin pass elongation of the reference steel strip and a first rolling force corresponding to the skin pass elongation; Perform skin-pass on the current steel strip to obtain a second rolling force of the current steel strip corresponding to the skin-pass elongation; Based on the first rolling force, determining whether the fluctuation amplitude of the second rolling force is within a third set range; If not, the current finishing elongation is adjusted until the fluctuation amplitude is within the third setting range.
6. The method according to claim 5, characterized in that The third setting interval is ≤10%.
7. The method according to claim 1, characterized in that The tensile strength of the high-strength steel is ≥780Mpa.
Citation Information
Patent Citations
Method of setting temperature of radiant tubes at heating section of annealing furnace
CN108467938A
Control method for annealing transition of high-strength steel plate
CN113430360A
Method and system for obtaining strip steel radiation coefficient of annealing furnace
CN113591276A
Dewing early warning method for strip steel plate roll warehouse
CN114113216A
Heating section strip steel thermometer measurement deviation evaluation method and device