Method for bioleaching chalcopyrite

Through the Fenton-like reaction, the passivation layer on the surface of chalcopyrite is destroyed, the biological leaching efficiency of chalcopyrite is improved, the problem of low biological leaching rate of chalcopyrite is solved, and efficient, economical and environmentally friendly leaching effect is achieved.

CN119061262AActive Publication Date: 2024-12-03INSTITUTE OF PROCESS ENGINEERING CHINESE ACADEMY OF SCIENCES

Patent Information

Application Number
CN202411189188.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-03
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

The low biological leaching rate of chalcopyrite causes the surface passivation layer to hinder charge transfer and leads to a decrease in the leaching rate. Existing methods such as adding Cl-, increasing the temperature or using Ag+ catalysts have problems such as high costs or difficult to achieve industrial application in technology.

Method used

Using Fenton-like reaction synergistic biological oxidation, the oxidation of monovalent copper and divalent iron on the surface of chalcopyrite is formed by regularly spraying hydrogen peroxide, forming a loose elemental sulfur cover layer, destroying the passivation layer, improving leaching efficiency, and not Control reaction conditions under the premise of affecting microbial growth.

Benefits of technology

It has achieved efficient biological leaching of chalcopyrite, which is low cost, simple operation and environmentally friendly, improves leaching efficiency and has the prospect of industrial application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005014559490000071
    Figure BDA0005014559490000071
  • Figure BDA0005014559490000081
    Figure BDA0005014559490000081
Patent Text Reader

Abstract

The invention provides a chalcopyrite bioleaching method which comprises the following steps: (1) chalcopyrite is crushed and built into an ore heap, and vertical pipes are buried in the ore heap; (2) spraying the ore heap with sulfuric acid, and then inoculating mineral leaching microorganisms to realize biological leaching heap operation; and (3) in the running process of the bioleaching heap, spraying a spraying liquid at the top of the ore heap at regular intervals, and adding hydrogen peroxide into the spraying liquid according to the copper ion concentration change condition. According to the method, the passivation layer on the surface of the chalcopyrite is eliminated and the regeneration of the passivation layer is hindered by using the Fenton-like reaction and the biological oxidation, so that the leaching efficiency of the chalcopyrite is improved, the efficient biological leaching of the chalcopyrite is realized, and the method is relatively low in cost, simple and convenient to operate and green and environment-friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hydrometallurgy, and specifically relates to a chalcopyrite bioleaching method, in particular to a chalcopyrite bioleaching method with high leaching efficiency. Background Art

[0002] Bio-heap leaching can directly utilize low-grade copper ore, avoiding the high-energy consumption and high-pollution steps of grinding, beneficiation and smelting in the mining and metallurgical process. It not only has low production costs and simple process operation, but also has no harmful flue gas emissions, and has obvious advantages in terms of economy and environmental protection. To date, nearly a quarter of the world's copper production has been obtained through bio-heap leaching. However, bio-heap leaching is currently mainly used to treat low-grade ores containing secondary copper sulfide ores such as chalcocite (Cu2S), while minerals containing primary copper sulfide ores such as chalcopyrite (CuFeS2) are currently difficult to achieve large-scale industrial application due to the slow bioleaching rate of copper. Chalcopyrite is an economically important primary copper sulfide ore, accounting for about 70% of the world's total copper resources. Realizing the bioleaching of low-grade chalcopyrite will produce economic benefits far greater than the use of secondary copper sulfide ores alone.

[0003] A large number of studies have confirmed that the reason for the low bioleaching rate of chalcopyrite is that after a certain stage of bioleaching, the passivation layer on the surface of chalcopyrite will hinder the direct contact between the solution and the chalcopyrite surface and hinder the charge transfer. This phenomenon is called surface passivation, which will cause the leaching rate to drop sharply or even stop. The current methods for removing or reducing the surface passivation of chalcopyrite include the following methods:

[0004] Adding Cl to the bioleaching system - , using Cl - The high permeability of Cl promotes the dissolution of chalcopyrite and inhibits the formation of passive film. - Too high a concentration will affect the growth of microorganisms, inhibit their sulfur oxidation ability, and also affect subsequent extraction and electrolysis processes, causing equipment corrosion and a decline in the quality of metallic copper products.

[0005] Increasing the temperature or using bioleaching and ozone oxidation staged reaction methods can remove the passivation film formed by chalcopyrite in bioleaching and achieve efficient leaching of chalcopyrite. However, for large-scale heap leaching processes, increasing the temperature or performing staged leaching is technically difficult to achieve, and there is no report on the industrial application of such methods.

[0006] Add Ag + As a catalyst, it can significantly increase the bioleaching rate of chalcopyrite. + The catalytic effect is good and the impact on microorganisms is small. When bioleaching is carried out in a stirred tank, Ag +The catalytic effect of can increase the leaching rate of chalcopyrite to nearly 90%, and can also increase the leaching rate of copper by more than 1 times in the simulated biological heap leaching process. However, silver is expensive, and in actual biological heap leaching, it will form iron silver alum precipitation and be lost, resulting in increased production costs.

[0007] Therefore, how to provide a method that can destroy the passivation film on the surface of chalcopyrite and improve the biological oxidation efficiency of chalcopyrite has become an urgent problem to be solved. Summary of the invention

[0008] In view of the shortcomings of the prior art, the object of the present invention is to provide a method for bioleaching chalcopyrite, and in particular to provide a method for bioleaching chalcopyrite with high leaching efficiency. The method provided by the present invention utilizes a Fenton-like reaction in coordination with bio-oxidation to eliminate the passivation layer on the surface of chalcopyrite and hinder the regeneration of the passivation layer, thereby improving the leaching efficiency of chalcopyrite, achieving efficient bioleaching of chalcopyrite, and having low cost, simple operation, and green environmental protection.

[0009] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0010] The present invention provides a method for bioleaching chalcopyrite, which comprises the following steps:

[0011] (1) crushing the chalcopyrite into an ore pile and burying a vertical pipe in the ore pile;

[0012] (2) Spraying the ore pile with sulfuric acid and then inoculating leaching microorganisms to achieve biological leaching operation;

[0013] (3) During the operation of the bioleaching pile, a spray liquid is sprayed regularly on the top of the ore pile, and hydrogen peroxide is added to the spray liquid according to the change in copper ion concentration.

[0014] The method adds H2O2 without affecting the normal growth of leaching microorganisms, utilizes the Fenton-like reaction to oxidize the monovalent copper and divalent iron on the surface of the chalcopyrite, the copper is leached first, and the sulfur forms a loose elemental sulfur covering layer, which reduces the hindering effect on the biological leaching process; the strong oxidizing property of the Fenton-like reaction itself is also conducive to the oxidation and dissolution of sulfur, destroying the already formed passivation covering layer, thereby achieving the purpose of hindering the regeneration of the passivation layer and eliminating the passivation layer on the surface of the chalcopyrite, and at the same time can cooperate with the biological oxidation effect to improve the leaching efficiency of the chalcopyrite, providing an economically feasible, easy-to-operate, energy-saving and environmentally friendly method for enhancing the biological leaching of chalcopyrite.

[0015] Preferably, the upper portion of the vertical pipe in step (1) is not lower than the top of the ore pile, and the lower portion is at least 30 cm higher than the bottom of the ore pile.

[0016] Preferably, the density of the vertical pipes in the ore pile in step (1) is 8-10 pipes / m 2, for example 8 pieces / m 2 , 9 pieces / m 2 or 10 pieces / m 2 .

[0017] Preferably, the concentration of sulfuric acid in step (2) is 0.04-0.08 mol / L, such as 0.04 mol / L, 0.05 mol / L, 0.06 mol / L, 0.07 mol / L or 0.08 mol / L, but is not limited to the above-listed values. Other values ​​not listed within the above numerical range are also applicable.

[0018] Preferably, the spraying rate of sulfuric acid in step (2) is 1-2 L / m 3 , for example 1L / m 3 , 1.1L / m 3 , 1.2L / m 3 , 1.3L / m 3 , 1.4L / m 3 , 1.5L / m 3 , 1.6L / m 3 , 1.7L / m 3 、1.8L / m 3 , 1.9L / m 3 or 2L / m 3 The above values ​​are not limited to the above values. Other values ​​not listed in the above value range are also applicable.

[0019] Preferably, the leaching microorganisms in step (2) include Acidithiobacillus ferrooxidans and Acidithiobacillus thiooxidans;

[0020] Preferably, after the inoculation of the leaching microorganisms in step (2), the initial density of the leaching microorganisms is 1×10 6 -1×10 8 Pieces / mL.

[0021] Preferably, the regular spraying of the spray liquid in step (3) is specifically performed once every 7-10 days, and the total amount of each spraying is 800-1200 mL, for example 800 mL, 900 mL, 1000 mL, 1100 mL or 1200 mL, but is not limited to the values ​​listed above, and other values ​​not listed within the above numerical range are also applicable.

[0022] Preferably, the step (3) of adding hydrogen peroxide to the spray liquid according to the change in copper ion concentration is specifically as follows:

[0023] Detect the copper ion concentration in the heap leachate. When the copper ion concentration rises slowly and the microbial density is greater than 1×10 6 When the concentration of iodine / mL was 0.1, hydrogen peroxide was added to the spray solution.

[0024] Preferably, the mass fraction of hydrogen peroxide added to the spray liquid in step (3) is 0-0.5%, but excluding 0.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] The invention provides a method for bioleaching chalcopyrite. H2O2 is added without affecting the normal growth of leaching microorganisms, and monovalent copper and divalent iron on the surface of the chalcopyrite are oxidized by using a Fenton-like reaction. Copper is leached first, and sulfur forms a loose elemental sulfur covering layer, which reduces the hindering effect on the bioleaching process. The strong oxidizing property of the Fenton-like reaction itself is also conducive to the oxidation and dissolution of sulfur, destroying the formed passivation covering layer, thereby achieving the purpose of hindering the regeneration of the passivation layer and eliminating the passivation layer on the surface of the chalcopyrite. At the same time, it can cooperate with the biological oxidation effect to improve the leaching efficiency of the chalcopyrite, and provides an economically feasible, easy-to-operate, energy-saving and environmentally friendly method for strengthening bioleaching of chalcopyrite. DETAILED DESCRIPTION

[0027] In order to further explain the technical means and effects adopted by the present invention, the technical solution of the present invention is further described below in conjunction with the preferred embodiments of the present invention, but the present invention is not limited to the scope of the embodiments.

[0028] In the example below, the chalcopyrite comes from a mine in Diqing, Yunnan.

[0029] Example 1

[0030] This embodiment provides a method for bioleaching chalcopyrite, and the specific steps are as follows:

[0031] (1) Chalcopyrite bio-heap leaching. The ore is crushed and piled up, and a certain number of vertical pipes are buried so that part of the spray liquid can directly reach the bottom of the ore pile. The vertical pipe density is 9 pipes / m 2 The inner diameter of the vertical pipe is 2 cm, and holes are opened on the side of the pipe. Four holes are opened around the pipe every 10 cm, and the hole diameter is 0.5 cm. The upper part of the vertical pipe is not lower than the top of the ore pile, and the lower part of the vertical pipe is 30 cm away from the bottom;

[0032] (2) After spraying with 0.046 mol / L dilute sulfuric acid (1.5 L / m 3 ), inoculated with acidithiobacillus ferrooxidans (At.f) and Thiobacillus thiooxidans (Tt) (inoculation ratio 1:1), and the initial density of leaching microorganisms was 1×10 7 / mL until the microorganisms are colonized in the heap and the bioleaching heap operates stably;

[0033] (3) Every 10 days, spray with 0.5% H2O2 at a flow rate of 100 mL / min for 10 min.

[0034] (4) Continuously monitor the microbial density and copper ion concentration in the ore pile. When the microbial density in the system is higher than 1×10 6 / mL, and the copper ion concentration growth rate slowed down, 0.5% H2O2 was used to spray at a flow rate of 100mL / min for 10min; when the microbial density in the system was lower than 1×10 6 / mL, stop adding hydrogen peroxide to the spray liquid.

[0035] Example 2

[0036] This embodiment provides a method for bioleaching chalcopyrite, and the specific steps are as follows:

[0037] (1) Chalcopyrite bioleaching. The ore is crushed and piled up, and a certain number of vertical pipes are buried so that part of the spray liquid can directly reach the bottom of the ore pile. The vertical pipe density is 8 pipes / m 2 The inner diameter of the vertical pipe is 2 cm, and holes are opened on the side of the pipe. Four holes are opened around the pipe every 10 cm, and the hole diameter is 0.5 cm. The upper part of the vertical pipe is not lower than the top of the ore pile, and the lower part of the vertical pipe is 30 cm away from the bottom;

[0038] (2) After spraying with 0.04 mol / L dilute sulfuric acid (1 L / m 3 ), inoculated with acidithiobacillus ferrooxidans (At.f) and Thiobacillus thiooxidans (Tt) (inoculation ratio 1:1), and the initial density of leaching microorganisms was 1×10 6 / mL until the microorganisms are colonized in the heap and the bioleaching heap operates stably;

[0039] (3) Spray with 0.5% H2O2 at a flow rate of 80 mL / min for 10 min every 7 days.

[0040] (4) Continuously monitor the microbial density and copper ion concentration in the ore pile. When the microbial density in the system is higher than 1×10 6 / mL, and the copper ion concentration growth rate slowed down, 0.5% H2O2 was used to spray at a flow rate of 80mL / min for 10min; when the microbial density in the system was lower than 1×10 6 / mL, stop adding hydrogen peroxide to the spray liquid.

[0041] Example 3

[0042] (1) Chalcopyrite bioleaching. The ore is crushed and piled up, and a certain number of vertical pipes are buried so that part of the spray liquid can directly reach the bottom of the ore pile. The density of the vertical pipes is 10 / m 2 The inner diameter of the vertical pipe is 2 cm, and holes are opened on the side of the pipe. Four holes are opened around the pipe every 10 cm, and the hole diameter is 0.5 cm. The upper part of the vertical pipe is not lower than the top of the ore pile, and the lower part of the vertical pipe is 30 cm away from the bottom;

[0043] (2) After spraying with 0.08 mol / L dilute sulfuric acid (2L / m 3 ), inoculated with acidithiobacillus ferrooxidans (At.f) and Thiobacillus thiooxidans (Tt) (inoculation ratio 1:1), and the initial density of leaching microorganisms was 1×10 8 / mL until the microorganisms are colonized in the heap and the bioleaching heap operates stably;

[0044] (3) Spray with 0.5% H2O2 at a flow rate of 120 mL / min for 10 min every 8 days.

[0045] (4) Continuously monitor the microbial density and copper ion concentration in the ore pile. When the microbial density in the system is higher than 1×10 6 / mL, and the copper ion concentration growth rate slowed down, 0.5% H2O2 was used to spray at a flow rate of 120mL / min for 10min; when the microbial density in the system was lower than 1×10 6 / mL, stop adding hydrogen peroxide to the spray liquid.

[0046] Example 4

[0047] This embodiment provides a method for bioleaching chalcopyrite. The specific steps are similar to those in the method of Embodiment 1, with the only difference being that 1% H2O2 is added in steps (3) and (4).

[0048] Example 5

[0049] This embodiment provides a method for bioleaching chalcopyrite. The specific steps are similar to those of the method in Example 1, with the only difference being that 1.5% H2O2 is added in steps (3) and (4).

[0050] Example 6

[0051] This embodiment provides a method for bioleaching chalcopyrite. The specific steps are similar to those in the method of Embodiment 1, with the only difference being that 2% H2O2 is added in steps (3) and (4).

[0052] Example 7

[0053] This embodiment provides a method for bioleaching chalcopyrite. The specific steps are similar to those of the method in Embodiment 1, with the only difference being that in step (3), spraying is performed once every 20 days.

[0054] Example 8

[0055] This embodiment provides a method for bioleaching chalcopyrite. The specific steps are similar to those of the method in Embodiment 1, with the only difference being that in step (3), spraying is performed once every 30 days.

[0056] Comparative Example 1

[0057] This comparative example provides a method for bioleaching chalcopyrite. The specific steps are similar to those in Example 1, except that H2O2 is not added in steps (3) and (4).

[0058] Effect test:

[0059] The chalcopyrite leaching efficiency in the methods of Examples 1-8 and Comparative Example 1 was calculated using the following formula:

[0060] Leaching rate = Cu in leachate 2+ Concentration / (total mass of leached ore × copper mass percentage);

[0061] The results are as follows:

[0062]

[0063]

[0064] From the above data, it can be found that the method of the present invention using Fenton-like reaction to enhance chalcopyrite bioleaching can achieve efficient leaching of chalcopyrite, is economically feasible, easy to operate, and has prospects for industrial application; by comparing Examples 1-6, it can be found that the present invention achieves an effective balance between the destruction of the passivation coating and the impact on microorganisms by controlling the amount of hydrogen peroxide added and the spraying cycle, thereby further improving the chalcopyrite leaching efficiency; by comparing Example 1 and Comparative Example 1, it can be found that the present invention effectively improves the chalcopyrite leaching efficiency by adopting Fenton-like reaction in coordination with biological oxidation.

[0065] The applicant declares that the present invention illustrates the method for bioleaching chalcopyrite of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

[0066] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0067] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

Claims

1. A method for bioleaching chalcopyrite, characterized in that: The method comprises the following steps: (1) crushing the chalcopyrite into an ore pile and burying a vertical pipe in the ore pile; (2) Spraying the ore pile with sulfuric acid and then inoculating leaching microorganisms to achieve biological leaching operation; (3) During the operation of the bioleaching pile, a spray liquid is sprayed regularly on the top of the ore pile, and hydrogen peroxide is added to the spray liquid according to the change in copper ion concentration.

2. The method according to claim 1, characterized in that The upper part of the vertical pipe in step (1) is not lower than the top of the ore pile, and the lower part is at least 30 cm higher than the bottom of the ore pile.

3. The method according to claim 1 or 2, characterized in that The density of the vertical pipes in the ore pile in step (1) is 8-10 pipes / m 2 ; Preferably, the vertical pipe in step (1) has a hole on its side.

4. The method according to any one of claims 1 to 3, characterized in that The concentration of sulfuric acid in step (2) is 0.04-0.08 mol / L.

5. The method according to any one of claims 1 to 4, characterized in that The spraying amount of sulfuric acid in step (2) is 1-2 L / m 3 .

6. The method according to any one of claims 1 to 5, characterized in that The leaching microorganisms in step (2) include Acidithiobacillus ferrooxidans and Acidithiobacillus thiooxidans; Preferably, after the inoculation of the leaching microorganisms in step (2), the initial density of the leaching microorganisms is 1×10 6 -1×10 8 Pieces / mL.

7. The method according to any one of claims 1 to 6, characterized in that The regular spraying of the spray liquid in step (3) is specifically performed once every 7-10 days, and the total amount of each spraying is 800-1200 mL.

8. The method according to any one of claims 1 to 7, characterized in that The specific method of adding hydrogen peroxide to the spray liquid according to the change of copper ion concentration in step (3) is as follows: Detect the copper ion concentration in the heap leachate. When the copper ion concentration rises slowly and the microbial density is greater than 1×10 6 When the concentration of iodine / mL was 0.1, hydrogen peroxide was added to the spray solution.

9. The method according to any one of claims 1 to 8, characterized in that The mass fraction of hydrogen peroxide added to the spray liquid in step (3) is 0-0.5%, but excluding 0.

Citation Information

Patent Citations

  • Method for removing heavy metals in excess sludge by bioleaching-similar Fenton oxidative coupling

    CN101891358A

  • Method for biologically leaching heavy metal from heavy metal-contained waste based on pH and potential co-regulation

    CN104862474A

  • Method for treating difficult-to-treat gold concentrates by ozone oxidization and microbial oxidation

    CN109112306A

  • Bacterial leaching of minerals

    EP0004431A1

  • Process for leaching copper from copper sulfide using bacteria

    US6168766B1

Cited By

  • Microbubble reinforced metal leaching system and method

    CN121653398A