Method for separating titanium from red mud
By carbide decalcification and acid leaching pretreatment in red mud, combined with microbubble flotation, the problems of high energy consumption and product impurities in red mud are solved, and the flotation recovery rate and efficiency of titanium are improved, thus achieving the Low cost titanium recycling and zero emissions of acids.
Patent Information
- Application Number
- CN202411185218.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
AI Technical Summary
The existing titanium recovery method in red mud has problems such as high energy consumption, complex process, and the joint entry of titanium with other non-target components into the leaching liquid, which affects product quality.
Carbonization decaling pretreatment and acid leaching pretreatment combined with microbubble flotation, by destroying the alkaline ore phase in red mud, reducing the pH value of the system, avoiding the acid leaching of titanium, and using microbubble flotation to increase the titanium Flotation recovery rate, reduce the dosage of the agent.
The separation efficiency of titanium in red mud is improved, energy consumption and chemical dosage is reduced, and low-cost titanium recycling is achieved. The acid-immersed pretreatment liquid can be reused, reducing the generation of waste acid.
Smart Images

Figure CN119061267A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of red mud hydrometallurgy, and in particular to a method for separating titanium from red mud. Background Art
[0002] Titanium and its alloys are widely used in the aerospace industry and the paint industry due to their excellent properties. However, the reserves of primary resources cannot meet the huge demand for this element. Therefore, it is of great significance to find secondary sources from low-grade ores and develop ways to recycle titanium. Red mud is the solid waste residue formed after alkaline hydrolysis of bauxite in the process of aluminum production. The titanium content is 1.9%-21.2%. Titanium minerals include perovskite, brookite, and ferro-titanium ore, which can be used as secondary raw materials for titanium separation.
[0003] At present, the main methods for recovering titanium from red mud include roasting pretreatment-slag leaching process, acid leaching process and combined metallurgy. Among them, the main problems faced by the roasting pretreatment-slag leaching process are high energy consumption, complex process, and a lot of useless residues generated in the treatment process; the red mud direct acid leaching process avoids the high energy consumption of roasting pretreatment, simplifies the process flow, and saves energy. However, the acid concentration used in the direct acid leaching process is relatively high. When leaching titanium acid, other non-target components such as Fe, Sc, Al, etc. enter the leaching solution together. The separation process is relatively complicated, which affects the quality of the final product. In addition, the amount of acid used as a leaching agent should be properly controlled to avoid the generation of too much waste acid. Summary of the invention
[0004] The present application provides a method for separating titanium from red mud to solve the following technical problem: how to improve the efficiency of separating titanium from red mud.
[0005] The present invention provides a method for separating titanium from red mud, comprising the following steps:
[0006] Carrying out carbonization and dealkalization pretreatment on red mud to obtain carbonized red mud;
[0007] The carbonized red mud is subjected to acid leaching pretreatment to obtain acid leaching pretreated red mud;
[0008] The acid leaching pretreated red mud is subjected to microbubble flotation to obtain titanium concentrate and red mud tailings.
[0009] Optionally, the carbonization and dealkalization pretreatment of red mud to obtain carbonized red mud specifically includes:
[0010] The red mud is placed in supercritical water or hot water, and carbon dioxide is introduced into the red mud to perform carbonization dealkalization pretreatment to obtain carbonized red mud.
[0011] Optionally, the liquid-to-solid ratio of the dealkalization pretreatment is 8 to 15:1, and the time of the dealkalization pretreatment is 15 min to 30 min.
[0012] Optionally, the carbonized red mud is subjected to acid leaching pretreatment to obtain acid leaching pretreated red mud, specifically comprising:
[0013] The carbonized red mud is immersed in a leaching solution for acid leaching pretreatment to obtain acid leaching pretreated red mud; the molar concentration of the leaching solution is 0.0005 mol / L to 0.01 mol / L.
[0014] Optionally, the parameters of the acid leaching pretreatment satisfy at least one of the following conditions: the liquid-to-solid ratio is 6 to 15:1; the acid leaching pretreatment temperature is 10°C to 70°C, and the acid leaching pretreatment time is 15min to 120min.
[0015] Optionally, the acid leaching pretreated red mud is subjected to microbubble flotation to obtain titanium concentrate and red mud tailings, specifically comprising:
[0016] adding an inhibitor and a collector to the acid leaching pretreated red mud to perform microbubble flotation to obtain titanium concentrate and red mud tailings;
[0017] Wherein, the inhibitor is oxalic acid and / or water glass, and the collector is a combined collector of sodium benzohydroxamate and modified phosphate.
[0018] Optionally, the molar ratio of the sodium benzohydroxamate to the modified phosphate ester is 6:1 to 1:3.
[0019] Optionally, based on weight, the inhibitor is used in an amount of 30 g / t to 60 g / t, and the collector is used in an amount of 50 g / t to 150 g / t.
[0020] Optionally, the amount of the collector is 100 g / t to 150 g / t by weight.
[0021] Optionally, the parameters of the microbubble flotation meet the following conditions: the slurry concentration is 20%; the pH value of the flotation system is 3-6.
[0022] Optionally, the pH value of the flotation system is 5-6.
[0023] Optionally, the microbubble flotation is a three-stage closed-circuit microbubble flotation, and the three-stage closed-circuit microbubble flotation includes one roughing selection and two fine selections.
[0024] The above technical solution provided by the present invention has the following advantages compared with the prior art:
[0025] The invention provides a method for separating titanium from red mud, which comprises the following steps: subjecting the red mud to carbonization dealkalization pretreatment, thereby destroying the structures of alkaline mineral phases such as hydrated garnet, tricalcium aluminate, cancrystal and sodalite in the red mud, making the mineral phases in the red mud unitary, simplified and destabilized, effectively reducing the pH value of the red mud system, and facilitating subsequent acid leaching treatment; after the pretreatment, filtering and separating to obtain carbonized red mud and alkaline filtrate; a part of the alkaline filtrate is used for subsequent flotation pH adjustment, and a part of the alkaline filtrate is neutralized with acidic water after flotation and then returned for carbonization pretreatment. The carbonized red mud is subjected to acid leaching pretreatment. On the one hand, the acid leaching pretreatment can leach out sodium, aluminum, silicon and iron in the red mud. At the same time, the titanium in the red mud does not enter the acid leaching pretreatment liquid, so the acid leaching of titanium can be avoided and the titanium loss can be reduced. On the other hand, the perovskite in the red mud can be separated from other minerals, which is beneficial to the subsequent flotation of titanium. After the acid leaching pretreatment is completed, the acid leaching pretreatment red mud and the acid leaching pretreatment liquid are obtained by solid-liquid separation, and the acid leaching pretreatment liquid can be reused as an acid leaching liquid. The acid leaching pretreatment red mud is subjected to microbubble flotation to obtain titanium concentrate and red mud tailings. The microbubble flotation process is more suitable for fine-grained minerals such as red mud because the bubbles are smaller, the collision frequency and adhesion probability between particles and bubbles are increased, and the microbubbles will increase the contact angle of the mineral surface, enhance the hydrophobicity of the mineral, reduce the difficulty of adhesion between mineral particles and bubbles, and increase the floatability of the mineral, that is, increase the flotation recovery rate, and the microbubbles play a secondary capture role on the surface of the mineral particles, which can reduce the dosage of the reagent, thereby realizing low-cost red mud titanium extraction. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0027] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0028] Figure 1 A flow chart of a method for separating titanium from red mud provided in some embodiments of the present application;
[0029] Figure 2 This is a flow chart of the method for separating titanium from red mud provided in Comparative Example 1 of the present application. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0031] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0032] In this application, in the absence of any contrary description, the terms including "including" and the like mean "including but not limited to". In this article, relational terms such as "first" and "second" and the like are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist, for example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "plurality" refers to two or more. "At least one", "the following at least one (individual)" or similar expressions thereof refer to any combination of these items, including any combination of singular (individual) or plural (individual). For example, "at least one of a, b, or c", or "at least one of a, b, and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or plural, respectively.
[0033] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0034] In a first aspect, the present invention provides a method for separating titanium from red mud, comprising the following steps:
[0035] Carrying out carbonization and dealkalization pretreatment on red mud to obtain carbonized red mud;
[0036] The carbonized red mud is subjected to acid leaching pretreatment to obtain acid leaching pretreated red mud;
[0037] The acid leaching pretreated red mud is subjected to microbubble flotation to obtain titanium concentrate and red mud tailings.
[0038] In the above-mentioned embodiment, the red mud carbonization and dealkalization pretreatment can effectively reduce the pH value of the red mud system, and the structures of alkaline mineral phases such as hydrated garnet, tricalcium aluminate, cancrystallinite and sodalite in the red mud are destroyed. The mineral phases in the red mud can be unified, simplified and destabilized, which is beneficial to the subsequent acid leaching treatment. The carbonized red mud is subjected to acid leaching pretreatment. On the one hand, the acid leaching pretreatment can leach out sodium, aluminum, silicon and iron in the red mud. At the same time, the titanium in the red mud does not enter the acid leaching pretreatment solution, so the acid leaching of titanium can be avoided and the titanium loss can be reduced. On the other hand, the perovskite in the red mud can be dissociated from other minerals, which is beneficial to the subsequent flotation of titanium. The microbubble flotation process is more suitable for fine-grained minerals such as red mud because the bubbles are smaller, the collision frequency and adhesion probability between particles and bubbles are increased, and the microbubbles can increase the contact angle of the mineral surface, enhance the hydrophobicity of the mineral, reduce the difficulty of adhesion between mineral particles and bubbles, and increase the floatability of the mineral, that is, increase the flotation recovery rate. In addition, the microbubbles play a secondary capture role on the surface of the mineral particles, which can reduce the dosage of reagents, thereby realizing low-cost red mud titanium extraction.
[0039] As an optional embodiment, the carbonization and dealkalization pretreatment of red mud to obtain carbonized red mud specifically includes:
[0040] The red mud is placed under supercritical water or hot water treatment, and carbon dioxide is introduced to react for a period of time to perform carbonization and dealkalization pretreatment to obtain carbonized red mud.
[0041] In the above embodiment, under supercritical water or hot water treatment, especially in supercritical water, the introduction of carbon dioxide can decompose cancrinite, hydrated garnet, etc. in red mud, which is conducive to subsequent acid leaching pretreatment at low temperature. At the same time, the use of carbon dioxide for dealkalization will not introduce new metal impurity ions. In addition, as a source of carbon dioxide, the flue gas discharged by the aluminum electrolysis industry or other waste gas from lime burning can also be used to save costs while reducing greenhouse gas emissions.
[0042] As an optional implementation manner, the liquid-to-solid ratio of the dealkalization pretreatment is 8 to 15:1, and the dealkalization pretreatment time is 15 min to 30 min.
[0043] In the above-mentioned embodiment, controlling the liquid-solid ratio of the dealkalization pretreatment helps to control the amount of carbon dioxide passed in. If the liquid-solid ratio is too low, the amount of liquid is too little, the carbon dioxide that can be dissolved in is reduced, and the cancrystal in the red mud, hydrated garnet, etc. cannot be completely decomposed, and the pH value of the system cannot be effectively reduced, which is not conducive to subsequent processes. If the liquid-solid ratio is too high, the amount of liquid is too much. Although the soluble carbon dioxide increases, after the same amount of carbon dioxide is passed in, the concentration of carbon dioxide decreases, resulting in a decrease in the dealkalization treatment effect. Exemplarily, the dealkalization pretreatment liquid-solid ratio can be 8: 1, 9: 1, 10: 1, 11: 1, 12: 1, 13: 1, 14: 1 or 15: 1. The pretreatment time can be adjusted according to the actual dealkalization situation. Exemplarily, the time can be 15min, 18min, 20min, 23min, 25min, 27min or 30min.
[0044] As an optional embodiment, the carbonized red mud is subjected to acid leaching pretreatment to obtain acid leaching pretreated red mud, specifically comprising:
[0045] The carbonized red mud is immersed in a leaching solution for acid leaching pretreatment, and then solid-liquid separation is performed to obtain acid leaching pretreated red mud; the molar concentration of the leaching solution is 0.0005 mol / L to 0.01 mol / L.
[0046] In the above embodiment, due to the dealkalization treatment, the gangue minerals and impurities in the red mud can be removed by using a relatively low concentration of acid, so that the leaching solution is enriched with aluminum, iron, silicon, etc., and the acid leaching pretreatment enriches titanium in the red mud to improve the titanium grade. At the same time, the perovskite is dissociated from other mineral phases, thereby improving the flotation efficiency of the perovskite.
[0047] As an optional implementation, the leaching solution is sulfuric acid and / or citric acid.
[0048] In the above embodiment, sulfuric acid and citric acid are selected to leach out as much aluminum, sodium, silicon, iron, etc. as possible from the red mud, while not leaching out titanium from the red mud.
[0049] As an optional implementation, the parameters of the acid leaching pretreatment meet the following conditions: the liquid-solid ratio is 6 to 15:1, the acid leaching pretreatment temperature is 10°C to 70°C, and the acid leaching pretreatment time is 15min to 120min.
[0050] In the above embodiment, the reason for controlling the liquid-to-solid ratio of the acid leaching pretreatment is that if the liquid-to-solid ratio is too high, there will be too much acid, which will easily dissolve the perovskite in the red mud and reduce the titanium recovery efficiency; if the liquid-to-solid ratio is too low, the acid will be too low, which may lead to incomplete dissolution of impurities in the red mud. Exemplarily, the liquid-to-solid ratio can be set to 6:1, 7:1, 8:1, 9:1, 10:1, 11:1, 12:1, 13:1, 14:1 or 15:1.
[0051] Due to the dealkalization treatment, the temperature of the acid leaching pretreatment does not need to be too high, and a temperature of 10°C to 70°C can be used. For example, the temperature of the acid leaching pretreatment can be set to 10°C, 20°C, 30°C, 40°C, 50°C, 60°C or 70°C.
[0052] The acid leaching pretreatment time can be adjusted according to actual needs, and the acid leaching pretreatment time can be adjusted by judging whether new metal ions are leached in the leaching solution. Exemplarily, the acid leaching pretreatment time can be set to 15min, 20min, 30min, 40min, 50min, 60min, 70min, 80min, 90min, 100min, 110min or 120min.
[0053] As an optional implementation manner, the acid leaching pretreated red mud is subjected to microbubble flotation to obtain titanium concentrate and red mud tailings, which specifically includes:
[0054] adding an inhibitor and a collector to the acid leaching pretreated red mud to perform microbubble flotation to obtain titanium concentrate and red mud tailings;
[0055] Wherein, the inhibitor is oxalic acid and / or water glass, and the collector is a combined collector of sodium benzohydroxamate and modified phosphate.
[0056] As an optional implementation manner, the molar ratio of the sodium benzohydroxamate to the modified phosphate ester is 6:1 to 1:3.
[0057] In the above embodiment, the collector used is a combination collector of sodium benzohydroxamate and modified phosphate because sodium benzohydroxamate has good selectivity in flotation, while the modified phosphate has strong collecting ability. When the two agents interact, an electron conjugation effect occurs between the electron-rich double bond in the modified phosphate ion and the electron-deficient benzene ring in the benzohydroxamate anion. The type of association complex generated by this effect and its spatial conformation are key factors affecting the flotation effect of the combined reagent, so the combination of the two can show a synergistic effect. The presence of the benzohydroxamate anion promotes the aggregation of the long hydrocarbon chain modified phosphate at the gas-liquid interface, and the fundamental reason for the aggregation of the modified phosphate on the surface of the aqueous solution is that the modified phosphate ion and the benzohydroxamate anion have an intermolecular interaction at the gas-liquid interface, generating an ion / molecular association complex, which is one of the main reasons affecting the surface tension of the combined reagent aqueous solution, the collecting ability of the combined reagent and the flotation behavior of the mineral.
[0058] Sodium benzohydroxamate is a highly efficient chelating flotation collector with good selectivity. The non-polar group of the molecule contains a benzene ring, and the polar group contains multiple bonded atoms that can act on the active sites of the mineral surface. The bonded atoms in the molecule can be chelated and coordinated with one or several active sites on the mineral surface and adsorbed on the mineral surface. At the same time, the hydrophobic phenyl group makes the target mineral exhibit good floatability, thereby achieving the purpose of capturing valuable minerals. In other words, the benzohydroxamate ion is chelated and coordinated on the surface of the perovskite and there are many ways of coordination. Therefore, the adsorption of the agent on the surface of the perovskite requires a large space. When sodium benzohydroxamate is added to the slurry, the agent can be chelated and coordinated on the surface of the perovskite in the best spatial geometric conformation, forming the initial hydrophobicity of the mineral surface. When the modified phosphate ester is continuously added to the slurry, the modified phosphate ester can be adsorbed on the active sites on the surface of the perovskite that are not covered by the benzohydroxamate ion in an interlaced adsorption manner, thereby further increasing the hydrophobicity of the mineral surface. However, the change in the ratio of the two reagents in the combination is by no means a simple replacement of the two reagents, but a certain interaction between the molecules and the generation of one or more new products, so that the effect of 1+1>2 can be achieved. Therefore, when sodium benzohydroxamate and modified phosphate are added to the slurry, in addition to being adsorbed on the mineral surface separately, the two will also undergo intermolecular association. The formation of the association complex can in turn further promote the adsorption of the reagents on the mineral surface, and the association complex generated by the intermolecular interaction has a stronger ability to capture perovskite than a single reagent. This is the main reason why the two reagents have a strong positive synergistic effect on the perovskite surface under this condition and the perovskite has good floatation in a wider range of reagent ratios.
[0059] However, these two agents may also compete for adsorption. The agent ions that are first adsorbed to the solid surface will produce greater steric hindrance to the later adsorbed agent, and the intermolecular complexes formed in a single liquid phase may not necessarily be adsorbed on the solid surface in the optimal spatial geometric conformation, resulting in differences in the grade and recovery rate of perovskite when the combined collectors are in different proportions. Therefore, choosing a suitable combination ratio of agents will have an important impact on the synergistic effect of the combined agents and the flotation behavior of perovskite. Exemplarily, the molar ratio of the sodium benzohydroxamate and the modified phosphate can be selected to be 3:1, 2:1, 1:1, 1:2 or 1:3.
[0060] As an optional embodiment, the molar ratio of the sodium benzohydroxamate to the modified phosphate is 3:1.
[0061] As an optional implementation manner, the dosage of the inhibitor is 30 g / t to 60 g / t, and the dosage of the collector is 50 g / t to 150 g / t.
[0062] As an optional implementation manner, the amount of the collector is 100 g / t to 150 g / t.
[0063] As an optional implementation, the parameters of the microbubble flotation meet the following conditions: the pulp concentration is 20%; the pH value of the flotation system is 3-6.
[0064] In the above embodiment, when the pH value of the flotation system is within this range, the Ti 4+ Mainly Ti(OH) 3+ and Ti(OH)2 2+ The combined collector is an anionic collector, so its active group can easily react with positively charged Ti(OH) 3+ and Ti(OH)2 2+ Combination occurs chemical adsorption, which has a better selective capture effect on perovskite and is more suitable for flotation extraction of titanium. The grade of titanium concentrate is higher and the flotation efficiency is high. When the pH value exceeds this value, the grade and recovery rate will decrease.
[0065] As an optional implementation, the pH value of the flotation system is 5-6.
[0066] In the above embodiment, the pH value of the flotation system is controlled to be 5-6, at which time the anion collector is more active. In this pH range, its active groups are easily combined with positively charged Ti(OH) 3+ and Ti(OH)2 2+ Combining and chemical adsorption occurs, which has a better selective capture effect on perovskite and is more suitable for flotation extraction of titanium.
[0067] As an optional implementation manner, the acid leaching pretreated red mud is subjected to microbubble flotation to obtain titanium concentrate and red mud tailings, which specifically includes:
[0068] The microbubble flotation is a three-stage closed-circuit microbubble flotation, and the three-stage closed-circuit microbubble flotation includes one roughing selection and two cleaning selections.
[0069] In the above embodiment, the three-stage closed-circuit microbubble flotation includes three flotation processes. The tailings are directly removed through a roughing process, and then the remaining perovskite continues to undergo two concentration processes. These two concentration processes can obtain high-grade titanium as much as possible through the inhibitory effect of the inhibitor and the collecting effect of the collector, thereby improving the flotation efficiency.
[0070] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to industry standards. If there is no corresponding industry standard, then the conditions recommended by the manufacturer are followed.
[0071] Example 1
[0072] This embodiment provides a method for separating titanium from red mud, the flow chart is as follows Figure 1 As shown, the following steps are included:
[0073] S1, select red mud with a titanium grade of 3.40%, firstly subject 500g of red mud to supercritical water carbonization dealkalization pretreatment, that is, under supercritical water treatment, introduce carbon dioxide into the red mud to carry out carbonization dealkalization pretreatment reaction, and pretreatment for 30min; after the dealkalization pretreatment is completed, filter and separate to obtain carbonized red mud and alkaline filtrate, wherein the alkaline filtrate can be used to adjust the pH in the flotation system and neutralize the acidic water generated after flotation;
[0074] S2, acid leaching pretreatment of the carbonized red mud: adding 0.0005 mol / L sulfuric acid to the carbonized red mud for acid leaching pretreatment, controlling the liquid-solid ratio to 7:1, the acid leaching pretreatment temperature to 40°C, and after acid leaching pretreatment for 60 minutes, obtaining acid leaching pretreated red mud and acid leaching pretreated liquid by solid-liquid separation; collecting the acid leaching pretreated liquid and using it as a leachate to repeat the acid leaching pretreatment of the red mud;
[0075] S3, subjecting the acid-pretreated red mud to three-stage closed-circuit microbubble flotation: the microbubble flotation in this embodiment includes one roughing and two fines. In each microbubble flotation, the pulp concentration is controlled to be 20%, the pH value of the flotation system is 5, 60 g / t of oxalic acid as an inhibitor is added, and after stirring for 1-3 minutes, 150 g / t of a combined collector is added, wherein the molar ratio of sodium benzohydroxamate to modified phosphate is 3:1, and after stirring for 1-3 minutes, aeration flotation is performed; the acidic water produced after the roughing and the last fine can be used to neutralize the alkaline filtrate produced in step S1, and re-participate in the carbonization dealkalization process.
[0076] The final flotation results of red mud tailings and titanium concentrate are shown in Table 1, and titanium concentrate with a titanium grade of 17.1% and a recovery rate of 60.07% was obtained.
[0077] Table 1 Test results of Example 1
[0078]
[0079] Example 2
[0080] The present embodiment provides a method for separating titanium from red mud, using the same red mud as in Example 1 as a raw material and the same separation method, the only difference being that, when the carbonized red mud is subjected to acid leaching pretreatment in step S2, 0.01 mol / L sulfuric acid is added to the carbonized red mud for acid leaching pretreatment, and the final flotation results of red mud tailings and titanium concentrate are shown in Table 2, obtaining red mud tailings and titanium concentrate with a grade of 18.6% and a recovery rate of 61.16%.
[0081] Table 2 Test results of Example 2
[0082]
[0083] Example 3
[0084] The present embodiment provides a method for separating titanium from red mud, using the same red mud as in Example 1 as a raw material and the same separation method, the only difference being that, when the carbonized red mud is subjected to acid leaching pretreatment in step S2, 0.003 mol / L sulfuric acid is added to the carbonized red mud for acid leaching pretreatment, and the final flotation results of red mud tailings and titanium concentrate are shown in Table 3, obtaining red mud tailings and titanium concentrate with a grade of 20.4% and a recovery rate of 62.02%.
[0085] Table 3 Test results of Example 3
[0086]
[0087] Example 4
[0088] The present embodiment provides a method for separating titanium from red mud, using the same red mud as in Example 1 as a raw material and a separation method, the difference being that when the carbonized red mud is subjected to acid leaching pretreatment in S2, 0.005 mol / L sulfuric acid is added to the carbonized red mud for acid leaching pretreatment, and the final flotation results of red mud tailings and titanium concentrate are shown in Table 4, obtaining red mud tailings and titanium concentrate with a grade of 21.45% and a recovery rate of 60.89%.
[0089] Table 4 Test results of Example 4
[0090]
[0091] Example 5
[0092] The present embodiment provides a method for separating titanium from red mud, using the same red mud as the raw material and the separation method as in Example 1, the difference being that when the carbonized red mud is subjected to acid leaching pretreatment in S2, 0.006 mol / L sulfuric acid is added to the carbonized red mud for acid leaching pretreatment, and the final flotation results of red mud tailings and titanium concentrate are shown in Table 5, obtaining red mud tailings and titanium concentrate with a grade of 20.8% and a recovery rate of 55.94%.
[0093] Table 5 Test results of Example 5
[0094]
[0095] Example 6
[0096] The present embodiment provides a method for separating titanium from red mud, using the same red mud as raw material and separation method as in Example 4, with the difference that when microbubble flotation is performed in S3, the molar ratio of the combined collector sodium benzohydroxamate and the modified phosphate ester used in the flotation is 1:1, and the final flotation results of red mud tailings and titanium concentrate are shown in Table 6, obtaining red mud tailings and titanium concentrate with a grade of 17.5% and a recovery rate of 69.35%.
[0097] Table 6 Test results of Example 6
[0098]
[0099] Example 7
[0100] The present embodiment provides a method for separating titanium from red mud, using the same red mud as raw material and separation method as in Example 4, with the difference that when microbubble flotation is performed in S3, the molar ratio of the combined collector sodium benzohydroxamate and the modified phosphate ester used in the flotation is 1:2, and the final flotation results of red mud tailings and titanium concentrate are shown in Table 7, obtaining red mud tailings and titanium concentrate with a grade of 15.92% and a recovery rate of 61.10%.
[0101] Table 7 Test results of Example 7
[0102]
[0103] Example 8
[0104] The present embodiment provides a method for separating titanium from red mud, using the same red mud as raw material and separation method as in Example 4, with the difference that when microbubble flotation is performed in S3, the molar ratio of the combined collector sodium benzohydroxamate and the modified phosphate ester used in the flotation is 1:3, and the final flotation results of red mud tailings and titanium concentrate are shown in Table 8, obtaining red mud tailings and titanium concentrate with a grade of 15.4% and a recovery rate of 53.94%.
[0105] Table 8 Test results of Example 8
[0106]
[0107] Example 9
[0108] The present embodiment provides a method for separating titanium from red mud, using the same red mud as raw material and separation method as in Example 4, with the difference that when microbubble flotation is performed in S3, the molar ratio of the combined collector sodium benzohydroxamate and the modified phosphate ester used in the flotation is 2:1, and the final flotation results of red mud tailings and titanium concentrate are shown in Table 9, obtaining red mud tailings and titanium concentrate with a grade of 19.87% and a recovery rate of 57.28%.
[0109] Table 9 Test results of Example 9
[0110]
[0111] Example 10
[0112] This embodiment provides a method for separating titanium from red mud, using the same red mud as in Example 4 as a raw material and a separation method, the difference being that when microbubble flotation is performed in S3, the pH value of the flotation system is 6, and the final flotation results of red mud tailings and titanium concentrate are shown in Table 10, obtaining red mud tailings and titanium concentrate with a grade of 20.2% and a recovery rate of 62.29%.
[0113] Table 10 Test results of Example 10
[0114]
[0115] Embodiment 11
[0116] This embodiment provides a method for separating titanium from red mud, using the same red mud as raw material and separation method as in Example 4, with the difference that when microbubble flotation is performed in S3, the pH value of the flotation system is 4, and the final flotation results of red mud tailings and titanium concentrate are shown in Table 11, obtaining red mud tailings and titanium concentrate with a grade of 19.5% and a recovery rate of 57.91%.
[0117] Table 11 Test results of Example 11
[0118]
[0119]
[0120] Example 12
[0121] This embodiment provides a method for separating titanium from red mud, using the same red mud as in Example 4 as a raw material and the same separation method, the only difference being that when microbubble flotation is performed in step S3, the pH value of the flotation system is 3, and the final flotation results of red mud tailings and titanium concentrate are shown in Table 12, obtaining red mud tailings and titanium concentrate with a grade of 18.8% and a recovery rate of 50.31%.
[0122] Table 12 Test results of Example 12
[0123]
[0124] Embodiment 13
[0125] This embodiment provides a method for separating titanium from red mud, using the same red mud as raw material and the same separation method as in Example 4, except that the amount of collector used in microbubble flotation in step S3 is 50 g / t. The final flotation results of red mud tailings and titanium concentrate are shown in Table 13, and red mud tailings and titanium concentrate with a grade of 18.35% and a recovery rate of 46.74% are obtained.
[0126] Table 13 Test results of Example 13
[0127]
[0128] Embodiment 14
[0129] This embodiment provides a method for separating titanium from red mud, using the same red mud as raw material and the same separation method as in Example 4, except that the amount of collector used in microbubble flotation in step S3 is 100 g / t. The results of the final flotation to produce red mud tailings and titanium concentrate are shown in Table 14, and red mud tailings and titanium concentrate with a grade of 21.1% and a recovery rate of 58.83% are obtained.
[0130] Table 14 Test results of Example 14
[0131]
[0132] Embodiment 15
[0133] This embodiment provides a method for separating titanium from red mud, which uses the same separation method as in Example 4, except that red mud with a titanium grade of 3.82% is selected. The final flotation results of red mud tailings and titanium concentrate are shown in Table 15, and red mud tailings and titanium concentrate with a grade of 22.1% and a recovery rate of 66.45% are obtained.
[0134] Table 15 Test results of Example 15
[0135]
[0136] Example 16
[0137] This embodiment provides a method for separating titanium from red mud, using the same separation method as in Example 4, except that the raw material in this embodiment is red mud with a titanium grade of 5.66%. The final flotation results of red mud tailings and titanium concentrate are shown in Table 16, and red mud tailings and titanium concentrate with a grade of 23.81% and a recovery rate of 69.80% are obtained.
[0138] Table 16 Test results of Example 16
[0139]
[0140] Comparative Example 1
[0141] The present comparative example provides a method for separating titanium from red mud. The method uses 500g of red mud with a titanium grade of 3.40% to directly perform three-stage closed-circuit microbubble flotation. The concentration of the flotation pulp is 20%. The pH value of the flotation system is adjusted to 5. After adding 60g / t of oxalic acid as an inhibitor and stirring for 1-3min, a combined collector of sodium benzohydroxamate and modified phosphate is added in a molar ratio of 3:1, and the amount of the collector is 150g / t. After stirring for 1-3min, aeration flotation is performed. The process flow chart is shown in the attached figure. Figure 2 As shown in Table 17, due to the direct use of the three-stage closed-circuit microbubble flotation process without dealkalization pretreatment and acid leaching pretreatment, the flotation red mud contains too many impurities. The flotation results are shown in Table 17, and only red mud tailings and titanium concentrate with a grade of 8.81% and a recovery rate of 52.69% are obtained.
[0142] Table 17 Test results of comparative example 1
[0143]
[0144] Comparative Example 2
[0145] This comparative example provides a method for separating titanium from red mud, which comprises the following steps:
[0146] S1, directly subjecting the red mud to acid leaching pretreatment: adding 0.0005 mol / L sulfuric acid to the red mud for acid leaching pretreatment, controlling the liquid-solid ratio to 7:1, the acid leaching pretreatment temperature to 40°C, and after acid leaching pretreatment for 60 minutes, obtaining acid leaching pretreated red mud and acid leaching pretreatment liquid by solid-liquid separation; collecting the acid leaching pretreatment liquid and using it as a leachate to repeat the acid leaching pretreatment of the red mud;
[0147] S2, subjecting the acid-pretreated red mud to three-stage closed-circuit microbubble flotation: the microbubble flotation in this embodiment includes one roughing and two fines. In each microbubble flotation, the pulp concentration is controlled to be 20%, the pH value of the flotation system is 5, 60 g / t of oxalic acid inhibitor is added, and after stirring for 1-3 minutes, 150 g / t of combined collector is added, wherein the molar ratio of sodium benzohydroxamate and modified phosphate is 3:1, and after stirring for 1-3 minutes, aeration flotation is performed; the acidic water produced after the roughing and the last fine can be used to neutralize the alkaline filtrate produced in step S1, and re-participate in the carbonization dealkalization process.
[0148] The final flotation results of red mud tailings and titanium concentrate are shown in Table 18. Since there is no dealkalization pretreatment and acid leaching is carried out directly, the acid concentration is low and other metal ions in the red mud cannot be leached out well, resulting in more red mud impurities in the flotation process. Therefore, the final flotation effect is poor, and only titanium concentrate with a titanium grade of 13.12% and a recovery rate of 52.85% is obtained.
[0149] Table 18 Test results of comparative example 2
[0150]
[0151] From the above examples and comparative examples, it can be seen that the titanium grade of the titanium concentrate finally obtained in the examples is as low as 15% and as high as more than 21%, but the titanium grade of the titanium concentrate finally obtained in the comparative example is less than 13.5%. It can be seen that the separation effect of titanium from red mud by the method for separating titanium from red mud provided by the present invention is better than the result of separation by directly using the flotation method. In addition, in the acid leaching pretreatment process used in the present invention, the lowest acid concentration can reach 0.0005 mol / L, which improves the separation effect while reducing the use of acid.
[0152] The present invention also pre-treats red mud with three different titanium grades to flotate and separate titanium, and obtains the following results: pre-treating red mud with a grade of 5% to 6% to flotate and separate titanium, and a titanium concentrate with a grade of 23.81% and a recovery rate of 69.80% can be obtained; pre-treating red mud with a grade of 3.5% to 4% to flotate and separate titanium, and a titanium concentrate with a grade of 22.1% and a recovery rate of 66.45% can be obtained; pre-treating red mud with a grade of 3% to 3.5% to flotate and separate titanium, and a titanium concentrate with a grade of 21.45% and a recovery rate of 60.89% can be obtained.
[0153] In summary, the method provided in the present invention can achieve high-grade titanium recovery for various red muds, and during the implementation process, the alkaline filtrate produced in the dealkalization process can not only be used to adjust the pH of the flotation system, but also be neutralized with the acidic water produced in the flotation process and returned to the dealkalization pretreatment operation to reduce the generation of wastewater; the acid leaching pretreatment liquid obtained in the acid leaching pretreatment process can be reused as a leaching liquid to achieve zero acid discharge. The carbon dioxide from the dealkalization treatment can also utilize the waste gas produced in the aluminum electrolysis process to reduce greenhouse gas emissions.
[0154] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for separating titanium from red mud, characterized in that: The following steps are involved: Carrying out carbonization and dealkalization pretreatment on red mud to obtain carbonized red mud; The carbonized red mud is subjected to acid leaching pretreatment to obtain acid leaching pretreated red mud; The acid leaching pretreated red mud is subjected to microbubble flotation to obtain titanium concentrate and red mud tailings.
2. The method for separating titanium from red mud according to claim 1, characterized in that: The red mud is subjected to carbonization and dealkalization pretreatment to obtain carbonized red mud, which specifically includes: placing red mud in supercritical water or hot water, and introducing carbon dioxide into the red mud to perform carbonization dealkalization pretreatment to obtain carbonized red mud; Wherein, the liquid-to-solid ratio of the dealkalization pretreatment is 8 to 15:1, and the time of the dealkalization pretreatment is 15 minutes to 30 minutes.
3. The method for separating titanium from red mud according to claim 1, characterized in that: The carbonized red mud is subjected to acid leaching pretreatment to obtain acid leaching pretreated red mud, specifically comprising: The carbonized red mud is immersed in a leaching solution for acid leaching pretreatment to obtain acid leaching pretreated red mud; the molar concentration of the leaching solution is 0.0005 mol / L to 0.01 mol / L.
4. The method for separating titanium from red mud according to claim 1, characterized in that: The method of subjecting the acid leaching pretreated red mud to microbubble flotation to obtain titanium concentrate and red mud tailings specifically includes: adding an inhibitor and a collector to the acid leaching pretreated red mud to perform microbubble flotation to obtain titanium concentrate and red mud tailings; Wherein, the inhibitor is oxalic acid and / or water glass, and the collector is a combined collector of sodium benzohydroxamate and modified phosphate.
5. The method for separating titanium from red mud according to claim 4, characterized in that: The molar ratio of the sodium benzohydroxamate to the modified phosphate is 6:1 to 1:
3.
6. The method for separating titanium from red mud according to claim 4, characterized in that: In terms of weight, the inhibitor is used in an amount of 30 g / t to 60 g / t, and the collector is used in an amount of 50 g / t to 150 g / t.
7. The method for separating titanium from red mud according to claim 6, characterized in that: The amount of the collector is 100 g / t to 150 g / t by weight.
8. The method for separating titanium from red mud according to claim 1 or 4, characterized in that: The microbubble flotation meets the following parameter conditions: The slurry concentration is 20%; The pH value of the flotation system is 3-6.
9. The method for separating titanium from red mud according to claim 8, characterized in that: The pH value of the flotation system is 5-6.
10. The method for separating titanium from red mud according to claim 1 or 4, characterized in that: The microbubble flotation is a three-stage closed-circuit microbubble flotation, and the three-stage closed-circuit microbubble flotation includes one roughing selection and two cleaning selections.
Citation Information
Cited By
Process method for preparing iron oxide red and extracting titanium dioxide from high-iron red mud
CN122079245A