Production method of foamed aluminum

By adding copper-plated carbon fiber and TiH2 to the foam aluminum production and controlling the mold cavity temperature, the problem of low yield strength of foam aluminum is solved, and high-performance production in normal temperature and high temperature environments is achieved, which simplifies operation and reduces costs.

CN119061288APending Publication Date: 2024-12-03CHINA NUCLEAR POWER ENGINEERING CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411195062.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing foam aluminum has low yield strength, making it difficult to maintain high performance in normal temperature and high temperature environments, and the production method is complex, costly, and poor environmental friendliness.

Method used

A foam aluminum production method is adopted, including alloy melt preparation, the addition of copper-plated carbon fibers and TiH2 foaming agent, and the precise control of the mold cavity temperature and stirring parameters to ensure uniform foaming and finished product quality of aluminum-silicon copper-zinc alloy melt. .

Benefits of technology

It improves the yield strength and yield rate of foam aluminum, reduces production costs, simplifies operating procedures, improves environmental friendliness, and maintains high performance in normal temperature and high and low temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061288A_ABST
    Figure CN119061288A_ABST
Patent Text Reader

Abstract

The invention discloses a production method of foamed aluminum, which comprises the following steps of: S1, preparing an alloy melt, namely melting an aluminum alloy containing silicon, copper and zinc at the temperature of between 700 and 710 DEG C, keeping the temperature, and continuously stirring to form an aluminum-silicon-copper-zinc alloy melt; s2, a first foaming agent is added into the aluminum-silicon-copper-zinc alloy melt and stirred, and the first foaming agent comprises copper-plated carbon fibers; s3, feeding a second foaming agent, namely adding the second foaming agent, and stirring; and S4, the aluminum-silicon-copper-zinc alloy melt containing the copper-plated carbon fibers after the second foaming agent is added is subjected to heat preservation and cooled to be in a semi-solid state, and then the aluminum-silicon-copper-zinc alloy melt is extruded into a mold. The foamed aluminum which can keep high yield strength in a normal-temperature environment and a high-low-temperature environment can be produced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of foam aluminum technology, and in particular to a method for producing foam aluminum. Background Art

[0002] Foamed aluminum is a multifunctional material with high porosity. It has the multifunctional composite characteristics of light weight, high toughness, crash resistance, high specific strength, high specific stiffness, flame retardant and heat insulation, vibration and noise reduction, corrosion resistance and electromagnetic shielding. It is widely used in the fields of electronics, communications, metallurgy, chemical industry, construction, transportation, aerospace, etc. The yield strength of foamed aluminum is an important factor affecting its energy absorption capacity. The greater the yield strength of foamed aluminum, the more energy can be absorbed per unit volume of foamed aluminum, which makes it easier to use it as an anti-collision energy absorption material.

[0003] The yield strength of existing foamed aluminum is generally low, and its yield strength under quasi-static compression is difficult to exceed 10MPa. Therefore, in a fixed space, the energy absorption performance of foamed aluminum materials is limited. For example, the prior art CN113774248A discloses a hierarchical density foamed aluminum production equipment and method. The production equipment includes a screw and a sleeve, and the sleeve is provided with a thickening aluminum liquid feeding port, a first foaming agent feeding device and a second foaming agent feeding device. The production method includes foaming, extrusion and molding; adding aluminum solution to the sleeve to stir and propel the aluminum liquid, and the front section of the sleeve is provided with a foaming section. The aluminum liquid added with the foaming agent completes foaming and expansion in the foaming section, and then enters the foaming bin.

[0004] Prior art CN109022880A discloses a rapid foaming device for foamed aluminum, comprising a foaming bin, one side of which is provided with a feed port, and the bottom of the foaming bin is provided with a melt extrusion nozzle, through which the aluminum liquid after foaming can be extruded; at least one side of the lower part of the foaming bin is connected to a foaming agent spray gun, and the spraying end of the foaming agent spray gun penetrates into the foaming bin, and an extrusion plate is provided in the foaming bin, and both ends of the extrusion plate are slidably connected to a slide rail, and the slide rail is fixed to the upper part of the inner wall of the foaming bin, and a cylinder is connected to the upper part of the extrusion plate, and the extrusion plate is driven to move up and down along the slide rail by controlling the telescopic action of the cylinder, so that the molten aluminum liquid after foaming in the foaming bin is extruded through the melt extrusion nozzle.

[0005] However, the current preparation methods of high yield strength aluminum foams all have shortcomings. In the preparation process of the infiltration casting method and the placeholder sintering method, a press is required to prepare the blank. The outer dimensions of the prepared aluminum foam are limited by the tonnage and table size of the press, and a special water dissolution container suitable for it is required. The operation is complicated, the molds are numerous, and the cost is high. The stir friction processing method requires a large amount of stir friction process, which includes the dispersion of the foaming agent and the connection between blanks with different characteristics, and requires high-temperature equipment to process, resulting in low processing efficiency and high cost. The chemical milling method requires the use of acid, alkali and other solutions, and requires special equipment to complete. It is not environmentally friendly and has a high cost. In addition, the temperature of the aluminum foam changes with the external temperature in the environment, and its yield strength will be greatly reduced at high temperatures.

[0006] Therefore, there is a need for an efficient, low-cost, high-performance method for producing foamed aluminum, which can maintain high yield strength under high and low temperature environments.

[0007] In view of the above technical problems, the present invention is specially introduced. Summary of the invention

[0008] The main purpose of the present invention is to provide a method for producing foamed aluminum, which is used to produce foamed aluminum that can maintain high yield strength both in normal temperature environment and in high and low temperature environment.

[0009] In order to achieve the above-mentioned purpose, the present invention proposes a method for producing foamed aluminum, comprising the following steps: an alloy melt preparation step, melting an aluminum alloy containing silicon, copper and zinc at a temperature of 700°C to 710°C, and starting continuous stirring after heat preservation to form an aluminum-silicon-copper-zinc alloy melt; a first foaming agent feeding step, adding a first foaming agent to the aluminum-silicon-copper-zinc alloy melt and stirring, the first foaming agent comprising copper-plated carbon fiber; a second foaming agent feeding step, adding a second foaming agent and stirring; a cooling and extrusion step, insulating the aluminum-silicon-copper-zinc alloy melt containing the copper-plated carbon fiber after adding the second foaming agent, cooling it to a semi-solid state, and then squeezing it into a mold.

[0010] Furthermore, the production method also includes a heating and taking-over step, wherein after the cooling and extrusion step S4 and before the mold cavity of the mold takes over, the bottom and side walls of the mold cavity are heated to different temperatures respectively.

[0011] Furthermore, in the heating receiving step, when receiving and producing foam aluminum with a relative mass of 10% to 15%, the receiving temperature of the bottom of the mold cavity is set at 590°C to 610°C; when receiving and producing foam aluminum with a relative mass of 15% to 20%, the receiving temperature of the bottom of the mold cavity is set at 640°C to 660°C; when receiving and producing foam aluminum with a relative mass of 20% to 30%, the receiving temperature of the bottom of the mold cavity is set at 740°C to 760°C.

[0012] Furthermore, in the heating step, the temperature of the side wall of the mold cavity is set to be 90° C. to 110° C. lower than the temperature of the bottom of the mold cavity.

[0013] Furthermore, in the first foaming agent feeding step, the mass proportion of the copper-coated carbon fiber in the aluminum-silicon-copper-zinc alloy melt does not exceed 2%.

[0014] Furthermore, in the first foaming agent feeding step, when the copper-plated carbon fiber is added, the temperature of the aluminum-silicon-copper-zinc alloy melt is between 580°C and 620°C.

[0015] Furthermore, in the first foaming agent feeding step, when the copper-plated carbon fiber is added, the stirring rate is set to 800 r / min and the stirring time is 180 s.

[0016] Furthermore, in the first foaming agent feeding step, pure calcium is added to the aluminum-silicon-copper-zinc alloy melt before adding the first foaming agent.

[0017] Furthermore, when the pure calcium is added, the stirring rate is set to 400 / min and the stirring time is 5 min.

[0018] Furthermore, the second foaming agent includes TiH2.

[0019] Furthermore, in the step of feeding the second foaming agent, the mass proportion of the TiH2 in the second foaming agent is 1.2%.

[0020] Furthermore, in the second foaming agent feeding step, when the second foaming agent is added, the stirring rate is set to 850 r / min and the stirring time is 300 s.

[0021] Furthermore, in the alloy melt preparation step, copper element accounts for 2% of the total mass of the aluminum-silicon-copper-zinc alloy melt, silicon element accounts for 5% of the total mass of the aluminum-silicon-copper-zinc alloy melt, and zinc element accounts for 2-4% of the total mass of the aluminum-silicon-copper-zinc alloy melt.

[0022] Furthermore, in the alloy melt preparation step, the holding time is 1 to 1.5 hours.

[0023] Furthermore, in the alloy melt preparation step, the stirring rate is set to 450 / min, and the stirring time is 10 to 12 min.

[0024] Furthermore, in the cooling extrusion step, the insulation temperature is first set to 600° C. for 6 minutes, and then the insulation temperature is increased to 710° C. for 1 minute.

[0025] By applying the technical solution of the present invention, at least the following beneficial effects are achieved:

[0026] 1. The production method of the present invention first prepares an aluminum-silicon-copper-zinc alloy melt, foams it, adds carbon fiber and evenly distributes it in the aluminum-silicon-copper-zinc alloy melt, further generates bubbles under the action of a TiH2 foaming agent, and finally grinds it under the action of a stirring propeller to generate fine bubbles. The production method improves the performance of foamed aluminum, improves the foaming uniformity and the yield rate, and produces a foamed aluminum that can maintain high yield strength both at room temperature and at high and low temperature environments.

[0027] 2. The production method of the present invention is designed to accurately control the receiving temperature of the bottom and side walls of the mold cavity when producing foam aluminum of different relative masses, so that the yield rate of foam aluminum is higher, and the quality and production efficiency of the produced foam aluminum products are improved.

[0028] 3. The production method of the present invention ensures the product quality of foam aluminum produced by this production method and the performance of maintaining high yield strength in high and low temperature environments by designing the stirring rate and stirring time of the stirring propeller in each step and adding detailed parameters such as the mass ratio of copper-plated carbon fiber and TiH2.

[0029] 4. The production method of the present invention adopts production equipment with a relatively simple structure, and compared with other current production methods for preparing high yield strength foam aluminum, it is simpler to operate, has good process control operability, high production efficiency, significantly reduced costs, high environmental friendliness, and a wider range of applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:

[0031] Figure 1 The main flow chart of the production method of the present invention is shown;

[0032] Figure 2 A schematic diagram of the production equipment used in the present invention before extrusion is shown;

[0033] Figure 3A schematic diagram showing the production equipment used in the present invention during extrusion;

[0034] Figure 4 The average density of the foamed aluminum prepared by the production method of the present invention at room temperature is 0.78 g / cm 3 Yield stress diagram of

[0035] Figure 5 The average density of the foamed aluminum prepared by the production method of the present invention at a high temperature of 300°C is 0.78 g / cm 3 Yield stress diagram of

[0036] Figure 6 The average density of the foamed aluminum prepared by the production method of the present invention is 0.78 g / cm at a low temperature of -40°C. 3 Yield stress diagram.

[0037] The above drawings include the following reference numerals:

[0038] 1. Conveying channel; 2. Foaming chamber; 3. Stirring propeller; 4. Alloy feeding device; 5. First foaming agent feeding device; 6. Second foaming agent feeding device; 7. Extrusion device; 8. Extrusion port; 9. Mold cavity; 10. Driving member; 11. Partition plate; 12. Extrusion tube; 13. Ventilation hole. DETAILED DESCRIPTION

[0039] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0040] The present invention is further described in detail below in conjunction with specific embodiments, and these embodiments cannot be understood as limiting the scope of protection claimed by the present invention. The term "including" when used indicates the existence of a feature, but does not exclude the existence or addition of one or more other features; the orientation or position relationship indicated by the terms "lateral", "upper", "lower", "front", "rear", "left", "right", "top", "bottom", "inside", "outside", etc. is based on the orientation or position relationship shown in the drawings, which is only for the convenience of description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention; in addition, the terms "first" and "second" are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance.

[0041] In the description, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected, or indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances. In addition, in the description of the present invention, unless otherwise specified, "plurality" means two or more.

[0042] Example:

[0043] The present invention provides a method for producing foamed aluminum, using a production device, combined with Figure 2 and Figure 3 As shown, the production equipment includes a conveying channel 1 and a foaming chamber 2 which are interconnected, a stirring propeller 3 is arranged in the conveying channel 1, an alloy feeding device 4, a first foaming agent feeding device 5 and a second foaming agent feeding device 6 are arranged in the conveying channel 1 from far to near the foaming chamber 2, an extrusion device 7 and an extrusion port 8 are arranged in the foaming chamber 2, and a mold is arranged outside the extrusion port 8. The mold has a plurality of mold cavities 9 for receiving the melt extruded from the extrusion port 8.

[0044] Preferably, the production equipment adopts a bilaterally symmetrical design, including two foaming chambers 2 separated by a partition plate 11, and the outer side of each foaming chamber 2 is connected to the conveying channel 1. The stirring propeller 3 adopts a screw, and the extrusion device 7 includes a connecting rod and an extrusion plate. The extrusion device 7 is driven by a driving member 10 to extrude in the foaming chamber 2. The driving member is preferably a cylinder. The outer side of the extrusion port 8 is connected to multiple extrusion tubes 12, which lead to different mold cavities 9 respectively, so as to improve production efficiency.

[0045] Combination Figure 1 As shown, the production method proposed by the present invention comprises the following steps:

[0046] In the alloy melt preparation step S1, aluminum alloy containing silicon, copper and zinc are melted at a temperature of 700°C to 710°C, kept warm and placed in the alloy feeding device 4 for 1 to 1.5 hours. The stirring propeller 3 starts to stir continuously and propel forward to form an aluminum-silicon-copper-zinc alloy melt.

[0047] Preferably, the copper element accounts for 2% of the total mass of the aluminum-silicon-copper-zinc alloy melt, the silicon element accounts for 5% of the total mass of the aluminum-silicon-copper-zinc alloy melt, and the zinc element accounts for 2-4% of the total mass of the aluminum-silicon-copper-zinc alloy melt. When adding the alloy feeding device 4, the stirring speed of the stirring propeller 3 is set to 450 / min, and the stirring time is 10-12min.

[0048] In the first foaming agent feeding step S2, preferably, pure calcium is added to the aluminum-silicon-copper-zinc alloy melt before the first foaming agent is added. Using pure calcium as a thickener can increase the viscosity of the aluminum-silicon-copper-zinc alloy melt, enhance the cohesion of the foamed aluminum, improve the pore size distribution of the foamed aluminum, and increase the strength of the foamed aluminum. Pure calcium can be added from the alloy feeding device 4 or the first foaming agent feeding device 5. When adding pure calcium, the stirring rate of the stirring propeller 3 is set to 400 / min, and the stirring time is 5min.

[0049] Afterwards, a first foaming agent including copper-coated carbon fiber is added to the first foaming agent feeding device 5. The copper-coated carbon fiber is added to the aluminum-silicon-copper-zinc alloy melt conveyed from the alloy feeding device 4 in the conveying channel 1 and stirred.

[0050] Preferably, the mass proportion of the copper-coated carbon fiber in the aluminum-silicon-copper-zinc alloy melt does not exceed 2%. When the copper-coated carbon fiber is added, the temperature of the aluminum-silicon-copper-zinc alloy melt is between 580°C and 620°C. When the copper-coated carbon fiber is added, the stirring rate of the stirring propeller 3 is set to 800r / min, and the stirring time is 180s. The copper-coated carbon fiber is evenly distributed in the aluminum-silicon-copper-zinc alloy melt.

[0051] In the second foaming agent feeding step S3, a second foaming agent is added to the second foaming agent feeding device 6, wherein the second foaming agent includes TiH2. Preferably, the mass proportion of TiH2 in the second foaming agent is 1.2%. When the second foaming agent is added, the stirring speed of the stirring propeller 3 is set to 850 r / min and the stirring time is 300 s. This allows the second foaming agent to uniformly act on the aluminum-silicon-copper-zinc alloy melt to generate bubbles.

[0052] The production method first prepares an aluminum-silicon-copper-zinc alloy melt, foams it, adds carbon fibers and evenly distributes them in the aluminum-silicon-copper-zinc alloy melt, further generates bubbles under the action of a TiH2 foaming agent, and finally grinds them into fine bubbles under the action of a stirring propeller. The production method improves the performance of foamed aluminum, increases the foaming uniformity and yield rate, and produces foamed aluminum that can maintain high yield strength both at room temperature and at high and low temperature environments.

[0053] In the cooling and extrusion step S4, the aluminum-silicon-copper-zinc alloy melt containing copper-plated carbon fiber after adding the second foaming agent is transported to the foaming chamber 2 for heat preservation. The heat preservation temperature is first set to 600° C. for 6 minutes, and then the heat preservation temperature is increased to 710° C. for 1 minute. Then it is cooled to a semi-solid state and extruded from the extrusion port 8 using the extrusion device 7.

[0054] In the heating successive step S5, the semi-solid aluminum-silicon-copper-zinc alloy melt is extruded through the extrusion port 8 into the mold cavity 9 of the mold, and the bottom and side walls of the mold cavity 9 are both provided with induction heating devices.

[0055] The foaming agent used in the foaming method to generate foam aluminum is basically TiH2, and the decomposition temperature of TiH2 is about 450°C, and then the decomposition speed reaches the fastest at 600°C, and the decomposition of TiH2 is basically completed when it reaches 730°C. Preferably, in the heating acceptance step S5, when receiving and producing foam aluminum with a relative mass of 10% to 15%, the receiving temperature at the bottom of the mold cavity 9 is set at 590°C to 610°C, when receiving and producing foam aluminum with a relative mass of 15% to 20%, the receiving temperature at the bottom of the mold cavity 9 is set at 640°C to 660°C, and when receiving and producing foam aluminum with a relative mass of 20% to 30%, the receiving temperature at the bottom of the mold cavity 9 is set at 740°C to 760°C.

[0056] In addition, the temperature of the side wall of the mold cavity 9 is set to be 90°C to 110°C lower than the temperature of the bottom of the mold cavity 9. When producing foamed aluminum of different relative qualities, the receiving temperatures of the bottom and side walls of the mold cavity are accurately controlled respectively, so that the yield rate of the foamed aluminum is higher, and the quality and production efficiency of the produced foamed aluminum products are improved.

[0057] In cooling forming step S6, cooling equipment such as water cooling pipes are also provided outside the mold cavity 9 to cool the semi-solid aluminum-silicon-copper-zinc alloy melt in the mold cavity to room temperature between 22-27°C. Finally, foamed aluminum with high yield strength under normal temperature, high temperature and low temperature environments can be obtained. In addition, after the mold cavity receives the semi-solid foamed aluminum, the isolation plate between the mold cavities is removed and the semi-solid foamed aluminum of different densities in different mold cavities is cooled and pressurized, wherein the temperature treatment method is to cool to the solidification temperature, at which time the foamed aluminum with high density gradient and the foamed aluminum with low density gradient are semi-solidly connected together, that is, to form a foamed aluminum plate with different density gradients, wherein the specific density of the foamed aluminum plate can be accurately controlled, and its specific density depends on the foaming density of the foamed aluminum received in the mold cavity, and the specific temperature can be adjusted according to the foamed aluminum solution actually received.

[0058] like Figure 4-6 As shown, Figure 4 The yield stress diagram of the foamed aluminum prepared by the method of the invention at room temperature with an average density of 0.78 g / cm3 is shown, and its yield stress can reach 27 MPa. Figure 5 The yield stress diagram of the foamed aluminum prepared by the method of the invention at a high temperature of 300°C with an average density of 0.78 g / cm3 is shown, and its yield stress can reach 22.5 MPa. Figure 6The yield stress diagram of the foamed aluminum prepared by the inventive method at a low temperature of -40°C with an average density of 0.78g / cm3 shows that its yield stress can reach 27.5MPa. After experimental verification, the foamed aluminum produced by this production method has high product quality and has the performance of maintaining high yield strength under high and low temperature environments. It also uses production equipment with a relatively simple structure, and compared with other current production methods for preparing foamed aluminum with high yield strength, it is easier to operate, has good process control operability, high production efficiency, significantly reduced costs, high environmental friendliness, and a wider range of applications.

[0059] In summary, from the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:

[0060] 1. The production method of the present invention first prepares an aluminum-silicon-copper-zinc alloy melt, foams it, adds carbon fiber and evenly distributes it in the aluminum-silicon-copper-zinc alloy melt, further generates bubbles under the action of a TiH2 foaming agent, and finally grinds it under the action of a stirring propeller to generate fine bubbles. The production method improves the performance of foamed aluminum, improves the foaming uniformity and the yield rate, and produces a foamed aluminum that can maintain high yield strength both at room temperature and at high and low temperature environments.

[0061] 2. The production method of the present invention is designed to accurately control the receiving temperature of the bottom and side walls of the mold cavity when producing foam aluminum of different relative masses, so that the yield rate of foam aluminum is higher, and the quality and production efficiency of the produced foam aluminum products are improved.

[0062] 3. The production method of the present invention ensures the product quality of foam aluminum produced by this production method and the performance of maintaining high yield strength in high and low temperature environments by designing the stirring rate and stirring time of the stirring propeller in each step and adding detailed parameters such as the mass ratio of copper-plated carbon fiber and TiH2.

[0063] 4. The production method of the present invention adopts production equipment with a relatively simple structure, and compared with other current production methods for preparing high yield strength foam aluminum, it is simpler to operate, has good process control operability, high production efficiency, significantly reduced costs, high environmental friendliness, and a wider range of applications.

[0064] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for producing foamed aluminum, characterized in that: The following steps are involved: Alloy melt preparation step S1, melting aluminum alloy containing silicon, copper and zinc at a temperature of 700° C. to 710° C., and then continuously stirring after heat preservation to form an aluminum-silicon-copper-zinc alloy melt; A first foaming agent feeding step S2, adding a first foaming agent to the aluminum-silicon-copper-zinc alloy melt and stirring the melt, wherein the first foaming agent comprises copper-plated carbon fiber; Second foaming agent feeding step S3, adding the second foaming agent and stirring; In the cooling extrusion step S4, the aluminum-silicon-copper-zinc alloy melt containing the copper-plated carbon fiber after adding the second foaming agent is kept warm, cooled to a semi-solid state, and then extruded into a mold.

2. The production method according to claim 1, characterized in that: The production method further comprises a heating and taking-over step S5, wherein after the cooling and extruding step S4 and before the mold cavity of the mold takes over, the bottom and side walls of the mold cavity are heated to different temperatures respectively.

3. The production method according to claim 2, characterized in that: In the heating receiving step S5, when receiving and producing foamed aluminum with a relative mass of 10% to 15%, the receiving temperature of the bottom of the mold cavity is set at 590°C to 610°C; when receiving and producing foamed aluminum with a relative mass of 15% to 20%, the receiving temperature of the bottom of the mold cavity is set at 640°C to 660°C; when receiving and producing foamed aluminum with a relative mass of 20% to 30%, the receiving temperature of the bottom of the mold cavity is set at 740°C to 760°C.

4. The production method according to claim 2 or 3, characterized in that: In the heating step S5, the temperature of the side wall of the mold cavity is set to be 90°C to 110°C lower than the temperature of the bottom of the mold cavity.

5. The production method according to claim 1, characterized in that: In the first foaming agent feeding step S2, the mass proportion of the copper-coated carbon fiber in the aluminum-silicon-copper-zinc alloy melt does not exceed 2%.

6. The production method according to claim 5, characterized in that: In the first foaming agent feeding step S2, when the copper-plated carbon fiber is added, the temperature of the aluminum-silicon-copper-zinc alloy melt is between 580°C and 620°C.

7. The production method according to claim 5, characterized in that: In the first foaming agent feeding step S2, when the copper-plated carbon fiber is added, the stirring rate is set to 800 r / min and the stirring time is 180 s.

8. The production method according to any one of claims 5 to 7, characterized in that: In the first foaming agent feeding step S2, pure calcium is added to the aluminum-silicon-copper-zinc alloy melt before adding the first foaming agent.

9. The production method according to claim 8, characterized in that: When the pure calcium was added, the stirring rate was set to 400 / min and the stirring time was 5 min.

10. The production method according to claim 1, characterized in that: The second blowing agent includes TiH2.

11. The production method according to claim 10, characterized in that: In the second foaming agent feeding step S3, the mass proportion of the TiH2 in the second foaming agent is 1.2%.

12. The production method according to claim 10, characterized in that: In the second foaming agent feeding step S3, when adding the second foaming agent, the stirring rate is set to 850 r / min and the stirring time is 300 s.

13. The production method according to claim 1, characterized in that: In the alloy melt preparation step S1, copper element accounts for 2% of the total mass of the aluminum-silicon-copper-zinc alloy melt, silicon element accounts for 5% of the total mass of the aluminum-silicon-copper-zinc alloy melt, and zinc element accounts for 2-4% of the total mass of the aluminum-silicon-copper-zinc alloy melt.

14. The production method according to claim 13, characterized in that: In the alloy melt preparation step S1, the holding time is 1 to 1.5 hours.

15. The production method according to claim 13, characterized in that: In the alloy melt preparation step S1, the stirring rate is set to 450 / min, and the stirring time is 10 to 12 minutes.

16. The production method according to claim 1, characterized in that: In the cooling extrusion step S5, the insulation temperature is first set to 600° C. for 6 minutes, and then the insulation temperature is increased to 710° C. for 1 minute.

Citation Information

Patent Citations

  • Foamed aluminum rapid foaming device

    CN109022880A

  • Hierarchical density foamed aluminum production equipment and method

    CN113774248A