Zinc-aluminum-magnesium alloy coating, hot-dip galvanized aluminum-magnesium coating steel plate and preparation method
By using zinc-aluminum-magnesium alloy plating in hot-dip aluminum-galvanized steel plates, the chemical composition and cooling speed are optimized, and the problem of the plating forming a thick dendritic aluminum-rich phase during solidification is solved, and the processing performance and surface quality of the plating are improved , achieving double improvements in corrosion resistance and forming capabilities.
Patent Information
- Application Number
- CN202411229439.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-12-03
AI Technical Summary
The dendritic aluminum-rich phase formed by the hot-dip aluminum-galvanized steel plate during solidification leads to poor plating processing performance, and a coarse and initial solidified Al phase may appear after adding magnesium, affecting the forming ability and surface quality of the plating.
The zinc-aluminum-magnesium alloy coating is used, and the chemical components include Mg: 2% to 7%, Al: 5% to 20%, Si: 0.05% to 1%, B: 0.001% to 0.1%, and the components and cooling speed are reasonably designed. Refine α-Al dendrites to reduce large binary eutectic structures and form optimized microstructures.
While maintaining the corrosion resistance of the coating, it significantly improves the processing and forming ability and surface quality of the coating, reduces the occurrence of cracks, and improves the overall performance of the coating.
Smart Images

Figure CN119061339A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of coating and plating technology, and in particular to a zinc-aluminum-magnesium alloy coating, a hot-dip zinc-aluminum-magnesium coated steel plate and a preparation method thereof. Background Art
[0002] In recent years, in order to improve the corrosion resistance of steel structures in the construction field, a wave of using hot-dip coated steel plates has emerged. Commonly used hot-dip coated steel plates include hot-dip galvanized steel plates, hot-dip aluminum-zinc coated steel plates, etc.
[0003] During the manufacturing process of hot-dip aluminum-zinc coated steel sheets, the molten aluminum-zinc coating will first form a dendritic aluminum-rich phase during the solidification process. Between these dendritic aluminum-rich phases, a zinc-rich eutectic structure will be formed, which will solidify last. Since the aluminum-rich phase growth morphology is complex and dendritic, it is difficult for corrosion to spread, so the corrosion rate is reduced, and the corrosion resistance of the coating is improved. However, this aluminum-zinc coating contains a large number of coarse aluminum-rich dendrites, which makes the coating processing performance poor. After processing, the coating is prone to cracks visible to the naked eye. At the same time, the surface of the coating also presents visible textures to the naked eye, which is not conducive to surface beautification in many occasions.
[0004] In order to maintain the corrosion resistance of the coating and improve the processing and forming ability of the coating, the aluminum in the coating can be reduced and an appropriate amount of magnesium can be added to improve the corrosion resistance and processing and forming ability. However, after adding magnesium, the initial solidified Al phase may still be formed. If the Al phase is too coarse, it will still lead to poor processing effect and poor surface quality. Summary of the invention
[0005] The present application provides a zinc-aluminum-magnesium alloy coating to solve the following technical problem: how to improve the processing and forming capability of the coating while maintaining the corrosion resistance of the coating.
[0006] In a first aspect, the present application provides a zinc-aluminum-magnesium alloy coating, wherein the chemical composition of the zinc-aluminum-magnesium alloy coating comprises, by mass fraction: Mg: 2% to 7%, Al: 5% to 20%, Si: 0.05% to 1%, B: 0.001% to 0.1%, and Zn.
[0007] Optionally, the Mg content of the zinc-aluminum-magnesium alloy coating is 3% to 5%, and the Al content of the zinc-aluminum-magnesium alloy coating is 8% to 15%.
[0008] Optionally, the chemical composition of the zinc-aluminum-magnesium alloy coating satisfies:
[0009] [Mg]=1617-1630 / (EXP(([Al]-320) / 69)+1)-x,
[0010] In the formula, [Mg] represents the mass fraction of Mg, [Al] represents the mass fraction of Al, and x is 0 to 1.5.
[0011] Optionally, the microstructure of the zinc-aluminum-magnesium alloy coating satisfies at least one of the following:
[0012] The area percentage of α-Al dendrites is ≤30%;
[0013] The length of the primary dendrite arm of α-Al dendrite is ≤100 μm;
[0014] The area percentage of blocky binary eutectic structure is ≤10%;
[0015] The equivalent diameter of the bulk binary eutectic structure is ≤100 microns.
[0016] In a second aspect, the present application provides a hot-dip galvanized aluminum-magnesium coated steel plate, which includes a steel substrate and a coating attached to at least a portion of the surface of the steel substrate; the coating includes the zinc-aluminum-magnesium alloy coating described in any one of the embodiments in the first aspect.
[0017] Optionally, an alloy layer is contained between the zinc-aluminum-magnesium coating and the steel substrate.
[0018] Optionally, the alloy layer is composed of Al-Fe system compounds and Mg-Si system compounds.
[0019] Optionally, the average thickness of the alloy layer is 0.03 μm to 1 μm.
[0020] In a third aspect, the present application provides a method for preparing a hot-dip galvanized aluminum-magnesium coated steel sheet, the method comprising:
[0021] heating the steel substrate;
[0022] Immersing the heated steel substrate into a plating solution containing the chemical components of the zinc-aluminum-magnesium alloy coating to form a coating, thereby obtaining a hot-dip zinc-aluminum-magnesium coated steel sheet;
[0023] The hot-dip galvanized aluminum-magnesium coated steel sheet is cooled to below 300° C. at a set cooling rate.
[0024] Optionally, the set cooling rate is >10K / s.
[0025] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0026] The present application provides a zinc-aluminum-magnesium alloy coating, wherein the composition of the zinc-aluminum-magnesium alloy coating includes, by mass fraction, Mg: 2% to 7%, Al: 5% to 20%, Si: 0.05% to 1%, B: 0.001% to 0.1%, and Zn. By rationally designing the composition of the zinc-aluminum-magnesium alloy coating, the α-Al dendrites are refined during the formation of the coating, the length of the primary dendrite arm of the α-Al dendrite is significantly reduced, and the bulk binary eutectic structure is reduced, so that the coating has improved processing and forming capabilities while maintaining corrosion resistance, and the surface quality is improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0028] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0029] Figure 1 A schematic diagram of a process for preparing a hot-dip galvanized aluminum-magnesium coated steel plate according to some embodiments of the present application; DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0031] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity and should not be understood as a rigid limitation on the scope of the present application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values within the range; for example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which applies regardless of the range; in addition, whenever a numerical range is indicated in this document, it is meant to include any cited numbers (fractions or integers) within the indicated range.
[0032] In this document, the terms including "including" and "including" mean "including but not limited to". Relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. "And / or" describes the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone; where A and B can be singular or plural. "At least one" means one or more, and "plurality" means two or more; "at least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single or plural items; for example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple. Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0033] In a first aspect, the present application provides a zinc-aluminum-magnesium alloy coating, wherein the chemical composition of the zinc-aluminum-magnesium alloy coating comprises, by mass fraction: Mg: 2% to 7%, Al: 5% to 20%, Si: 0.05% to 1%, B: 0.001% to 0.1%, and Zn.
[0034] In some embodiments, the Mg content of the zinc-aluminum-magnesium alloy coating is 3% to 5%, and the Al content of the zinc-aluminum-magnesium alloy coating is 8% to 15%.
[0035] The positive effect of controlling the Mg content to 2% to 7% is that the Mg element in the coating can significantly improve the atmospheric corrosion resistance of the coating. The mechanism is that the Mg in the coating will preferentially dissolve into the water film on the surface of the coating in the atmospheric environment, react with the dissolved carbon dioxide in the water film, and precipitate a dense protective film. This protective film can stably exist in a neutral and weakly alkaline environment, and can also cause the electrolyte solution on the surface of the coating to become a weakly alkaline solution, thereby improving the corrosion resistance of the coating. The Mg element in the coating preferentially combines with Zn to form a Mg-Zn compound, and then combines with Si to form a Mg-Si compound. If the Mg content is relatively high, large pieces of Mg-Zn compounds are likely to appear during hot dip plating. Mg-Zn compounds are brittle compounds that reduce the processing performance of the coating in the coating. The influence of large pieces of Mg-Zn compounds is particularly obvious. In the embodiment of the present application, the Mg content is preferably 3% to 5%. Exemplarily, the Mg content can be 2%, 3%, 4%, 5%, 7%, etc.
[0036] The positive effect of controlling the Al content to 5% to 20% is that the Al in the coating provides the coating with high-quality atmospheric corrosion resistance, because during the corrosion process, Al can form dense oxides and dense hydroxides on the surface. If the Al content in the coating is too little, the bonding between the coating and the steel plate will be very poor, making the coating unusable and reducing corrosion resistance; if the Al content in the coating is too much, a lot of coarse α-Al phases will be formed when the coating is formed. In the embodiment of the present application, the Al content is preferably 8% to 15%. Exemplarily, the Al content can be 5%, 7%, 10%, 15%, 20%, etc.
[0037] The positive effect of controlling the Si content to 0.05% to 1% is that Si can form compounds with elements to avoid the appearance of large Mg-Zn compounds and large binary eutectic structures. At the same time, Si can prevent the thickness of the alloy layer between the steel plate and the coating from being too thick, resulting in brittle cracks in the alloy layer itself. Too much Si will cause the precipitation of elemental Si particles in the coating, deteriorating the corrosion resistance of the coating. Exemplarily, the Si content can be 0.05%, 0.1%, 0.3%, 0.5%, 1%, etc.
[0038] The positive effect of controlling the B content to 0.001% to 0.1% is that B mainly interacts with α-Al dendrites in the coating. B can react with Al to form Al-B compound particles, which are first precipitated during the hot dip plating process to provide a nucleation core for α-Al, thereby refining the α-Al dendrites and significantly reducing the length of the primary dendrite arm of the α-Al dendrite. This is beneficial to improving the forming properties of the coating and improving the surface quality. Excessive addition of B will lead to the appearance of a large number of Al-B compound particles, which will weaken the role of Al in the coating and reduce the corrosion resistance of the coating. Exemplarily, the B content can be 0.001%, 0.005%, 0.03%, 0.05%, 0.1%, etc.
[0039] In some embodiments, the chemical composition of the zinc-aluminum-magnesium alloy coating satisfies:
[0040] [Mg]=1617-1630 / (EXP(([Al]-320) / 69)+1)-x,
[0041] In the formula, [Mg] represents the mass fraction of Mg, [Al] represents the mass fraction of Al, and x is 0 to 1.5.
[0042] By more accurately controlling the ratio of Al and Mg in the coating, the appearance of coarse α-Al and large binary eutectic structures can be minimized. Through a large number of experimental studies, it was found that when the mass fraction of Al and Mg in the coating satisfies: [Mg] = 1617-1630 / (EXP(([Al]-320) / 69)+1)-x, x is 0-1.5, a relatively ideal coating structure can be obtained. There is no obvious coarse α-Al phase and large binary eutectic structure in this coating. If x is less than 0, more large binary eutectic structures will appear; if x is greater than 1.5, more coarse α-Al will appear. Exemplarily, x can be 0.5, 0.8, 1, 1.2, 1.3, 1.5, etc.
[0043] In some embodiments, the microstructure of the zinc-aluminum-magnesium alloy coating satisfies at least one of the following:
[0044] The area percentage of α-Al dendrites is ≤30%;
[0045] The length of the primary dendrite arm of α-Al dendrite is ≤100 μm;
[0046] The area percentage of blocky binary eutectic structure is ≤10%;
[0047] The equivalent diameter of the bulk binary eutectic structure is ≤100 microns.
[0048] The positive effect of controlling the area percentage of α-Al dendrites on the coating surface to ≤30% and the length of the primary dendrite arm of α-Al dendrites to ≤100 microns: the processing performance of the coarse α-Al phase is poor, and it is easy to break during forming, causing cracks in the coating. For example, the area percentage of α-Al dendrites can be 20%, 25%, 27%, 28%, 30%, etc.; the length of the primary dendrite arm of α-Al dendrites can be 80 microns, 85 microns, 90 microns, 95 microns, 100 microns, etc.
[0049] The positive effect of controlling the area percentage of bulk binary eutectic structure ≤ 10% and the equivalent diameter of bulk binary eutectic structure ≤ 100 microns: large Mg-Zn compounds lead to accelerated local corrosion and reduced overall corrosion resistance of the coating. Large Mg-Zn compounds often appear together with η-Zn to form a binary eutectic structure. Exemplarily, the area percentage of bulk binary eutectic structure can be 2%, 5%, 7%, 8%, 10%, etc.; the equivalent diameter of bulk binary eutectic structure can be 80 microns, 85 microns, 90 microns, 95 microns, 100 microns, etc.
[0050] In a second aspect, the present application provides a hot-dip galvanized aluminum-magnesium coated steel plate, which includes a steel substrate and a coating attached to at least a portion of the surface of the steel substrate; the coating includes the zinc-aluminum-magnesium alloy coating described in any one of the embodiments in the first aspect.
[0051] The steel substrate is not particularly limited, and common steel plates such as hot-rolled steel plates and cold-rolled steel plates can be used. The type of steel is also not particularly limited, and for example, aluminum-killed steel, ultra-low carbon steel, and high-strength steel can be used.
[0052] In some embodiments, an alloy layer is contained between the zinc-aluminum-magnesium coating and the steel substrate.
[0053] In some embodiments, the alloy layer is composed of an Al-Fe system compound and a Mg-Si system compound.
[0054] In some embodiments, the alloy layer has an average thickness of 0.03 μm to 1 μm.
[0055] By forming an alloy layer composed of Fe-Al compounds and Mg-Si compounds between the coating and the steel substrate, the processing performance of the coating can be effectively improved and cracking of the coating during processing can be avoided.
[0056] The positive effect of controlling the thickness of the alloy layer to 0.03 μm to 1 μm: if the alloy layer is too thick, the brittleness of the coating will increase and the processing performance will decrease. For example, the thickness of the alloy layer can be 0.03 μm, 0.05 μm, 0.3 μm, 0.5 μm, 0.8 μm, 1 μm, etc.
[0057] Figure 1 A schematic flow chart of a method for preparing a hot-dip galvanized aluminum-magnesium coated steel plate provided in an embodiment of the present application.
[0058] See also Figure 1 In a third aspect, the present application provides a method for preparing a hot-dip galvanized aluminum-magnesium coated steel sheet, the method comprising:
[0059] S1, heating the steel substrate;
[0060] S2, immersing the heated steel substrate into a plating solution containing the chemical components of the zinc-aluminum-magnesium alloy coating to form a coating, thereby obtaining a hot-dip zinc-aluminum-magnesium coated steel sheet;
[0061] Heating usually needs to be carried out in a reducing atmosphere, such as nitrogen with a dew point of -60°C, in order to prevent oxides from forming on the surface of the coating. However, for some steel substrates with a high content of alloying elements, complex oxides may form on the surface even when heated in a reducing atmosphere. For such steel substrates, it may be necessary to first heat in an oxidizing atmosphere, such as nitrogen with a dew point of -10°C, or in nitrogen containing trace amounts of oxidizing gases, so that the alloying elements can be fully oxidized inside the steel, and then transferred to a reducing atmosphere for heating. Specific production process technology can be obtained through multiple attempts.
[0062] S3, cooling the hot-dip galvanized aluminum-magnesium coated steel plate to below 300° C. at a set cooling rate.
[0063] In some embodiments, the set cooling rate is >10K / s.
[0064] The positive effect of controlling the cooling rate to >10K / s: When the zinc-aluminum-magnesium coating solidifies, the α-Al phase is formed first, and then the binary eutectic structure composed of η-Zn and Mg-Zn compounds appears, and finally the ternary eutectic structure appears. In order to avoid the α-Al phase and the binary eutectic structure being too coarse, a relatively fast cooling rate of >10K / s is usually required during the formation stage of the α-Al phase and the binary eutectic structure. It is usually not necessary to control the upper limit of the cooling rate at this stage. However, if air blowing cooling is generally used, the upper limit of the cooling rate is 50K / s. Exemplarily, the set cooling rate can be 10K / s, 15K / s, 20K / s, 25K / s, 30K / s, 35K / s, etc.
[0065] The present application is further described below in conjunction with specific examples. The experimental methods in the following examples that do not specify specific conditions are usually measured according to industry standards; if there are no corresponding industry standards, they are carried out according to common international standards, conventional conditions, or conditions recommended by the manufacturer.
[0066] The steel substrate has a thickness of 2.5 mm and a width of 1000 mm, and the coating weight is 150 g / m2 on a single side. The composition, α-Al phase and cooling rate of the binary eutectic structure formation stage of the zinc-aluminum-magnesium alloy coating of the embodiment and the comparative example are shown in Table 1.
[0067] The composition of the coating can often be measured using the following methods:
[0068] First, an acid solution is obtained by stripping and dissolving the plating layer using an acid containing an inhibitor for inhibiting corrosion of a steel base (steel material). Next, the obtained acid solution is measured by ICP analysis to obtain the composition of the plating layer.
[0069] Table 1 Composition (wt%) of Zn-Al-Mg alloy coating, cooling rate (K / s) during the formation of α-Al phase and binary eutectic structure
[0070] Group Al Mg Si B Cooling rate 1617-1630 / (EXP(([Al]-320) / 69)+1)-[Mg] Example 1 5 3.5 0.05 0.1 20 0.29 Example 2 5 2.5 0.05 0.001 20 1.29 Example 3 15 6 1 0.1 40 0.38 Example 4 15 5 1 0.001 40 1.38 Comparative Example 1 2 1 0 0 5 2.08 Comparative Example 2 1 4 0 0 5 -1.15 Comparative Example 3 34 9 0 0 4 3.42 Comparative Example 4 30 12 0 0 4 -0.99 Example 5 20 7 0.05 0.005 30 0.81 Example 6 20 7 0.5 0.01 20 0.81 Example 7 10 4 0.1 0.05 15 1.04 Comparative Example 5 30 1 1.2 0 10 10.01 Comparative Example 6 40 1.5 2.3 2.1 10 13.19 Comparative Example 7 3 8 0 0.4 9 -4.69 Example 8 7 3 0.2 0.03 18 1.28 Example 9 7 3.3 0.6 0.005 19 0.98 Example 10 9 4.3 0.8 0.008 20 0.48 Embodiment 11 13 5.8 0.08 0.02 20 0.03 Comparative Example 8 18 7 0.1 0.03 1 0.23 Comparative Example 9 25 9 0 0 1 0.36 Comparative Example 10 25 10 0 0 40 -0.64 Comparative Example 11 30 14 0.8 0 40 -2.99 Comparative Example 12 3 0.2 0 1.2 1 3.11
[0071] Table 2 analyzes the characteristics of the α-Al phase and binary eutectic structure on the surface of the coatings of the embodiments and comparative examples.
[0072] The area ratio of various compounds on the coating surface can be measured by the following method:
[0073] A sample of 25 mm × 15 mm in size was prepared from the coated steel plate involved in this embodiment, and embedded in the resin in such a way that the surface of the sample became the observation surface. The surface of the coating was polished to eliminate the slight deformation of the coating surface, and the SEM image of the coating surface and the element distribution image based on EDS were obtained. The surface EDS mapping image of the coating was taken from 5 different samples with 1 field of view each, a total of 5 fields of view (magnification 1500 times: 60 μm × 50 μm / 1 field of view), and the area ratio of α-Al and blocky binary eutectic structure in the coating was calculated from the image.
[0074] The equivalent diameter D of the bulk binary eutectic structure=4*the area S of the bulk binary eutectic structure / the circumference l of the bulk binary eutectic structure.
[0075] The length of the primary dendrite arm of the α-Al phase on the coating surface can be measured by the following method:
[0076] A sample of 10 mm × 10 mm in size is prepared from the coated steel plate involved in the present embodiment. The sample is surface polished using electrolytic polishing technology to remove the surface stress layer. The sample is then subjected to EBSD observation to observe the surface of the coating. Different grains are identified based on the Al distribution using EBSD technology. The length of the primary dendrite arm of the α-Al phase in each grain is then counted. Five fields of view are collected for each sample, and a total of five samples are analyzed. The maximum value of the primary dendrite arm length of the α-Al phase in each field of view is calculated, and then the arithmetic mean of the maximum value of the primary dendrite arm length of the α-Al phase in all fields of view of the five samples is calculated.
[0077] The average thickness of the alloy layer between the coating and the steel substrate can be measured by the following method:
[0078] A sample of 10 mm×10 mm in size is prepared from the coated steel sheet involved in this embodiment, and a thin sample containing an alloy layer is cut from the coating layer using a focused ion beam process. The thickness of the thin sample should be suitable for transmission electron microscopy observation. The thin sample is then observed under a transmission electron microscope to measure the thickness of the alloy layer.
[0079] The corrosion resistance of the coating was evaluated using the JASO (M609-91) cyclic corrosion test. The cyclic corrosion test was performed for 100 cycles. If the corrosion weight loss of the coating reached 80g / m 2 , the corrosion resistance is evaluated as C. If the corrosion weight loss of the coating is 60g / m 2 ~80g / m 2 If the corrosion loss of the coating is between 50g / m 2 ~60g / m 2 If the corrosion weight loss of the coating does not exceed 50g / m 2 , the corrosion resistance is evaluated as AA.
[0080] Bend the coated steel plate 180° with a bending radius of 1mm. Then observe the cracks on the outer surface of the bent coating under a microscope. Count the total length of the cracks per unit area L (mm / cm 2 ). If L exceeds 10, the processing performance is evaluated as C. If L is between 7 and 10, the processing performance is evaluated as B. If L is not more than 7, the processing performance is evaluated as A.
[0081] White light interferometer is used to analyze the height of the unevenness on the coating surface. The Sa parameter is used to evaluate the unevenness height of the coating surface. If Sa reaches 5μm, the surface quality is evaluated as C. If Sa is 2-5μm, the surface quality is evaluated as B. If Sa is less than 2μm, the surface quality is evaluated as A.
[0082] Table 2 Characteristics of α-Al phase and binary eutectic structure on the coating surface
[0083]
[0084]
[0085] It can be seen from Tables 1 to 2 that the composition of the coatings of Examples 1 to 11 and the microstructure characteristics of the coating surfaces are all within the required range of the present invention, the total length of cracks per unit area is small, the corrosion resistance is good, and the surface quality is good.
[0086] One or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:
[0087] The hot-dip galvanized aluminum-magnesium coated steel sheet provided by the embodiment of the present invention has good corrosion resistance, excellent processing performance and good surface quality. In the microstructure of the coating, the area percentage of α-Al dendrites is ≤30%; the length of the primary dendrite arm of α-Al dendrites is ≤100 microns; the area percentage of block binary eutectic structure is ≤10%; and the equivalent diameter of the block binary eutectic structure is ≤100 microns.
[0088] The above is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. It will be apparent to those skilled in the art that various modifications to these embodiments are possible, and the general principles defined in the present application can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to these embodiments shown in the present application, but will conform to the widest scope consistent with the principles and novel features applied for by the present application.
Claims
1. A zinc-aluminum-magnesium alloy coating, characterized in that: Calculated by mass fraction, the chemical composition of the zinc-aluminum-magnesium alloy coating includes: Mg: 2% to 7%, Al: 5% to 20%, Si: 0.05% to 1%, B: 0.001% to 0.1%, and Zn.
2. The zinc-aluminum-magnesium alloy coating according to claim 1, characterized in that: The Mg content of the zinc-aluminum-magnesium alloy coating is 3% to 5%, and the Al content of the zinc-aluminum-magnesium alloy coating is 8% to 15%.
3. The zinc-aluminum-magnesium alloy coating according to claim 1, characterized in that: The chemical composition of the zinc-aluminum-magnesium alloy coating satisfies: [Mg]=1617-1630 / (EXP(([Al]-320) / 69)+1)-x, In the formula, [Mg] represents the mass fraction of Mg, [Al] represents the mass fraction of Al, and x is 0 to 1.
5.
4. The zinc-aluminum-magnesium alloy coating according to any one of claims 1 to 3, characterized in that: The microstructure of the zinc-aluminum-magnesium alloy coating satisfies at least one of the following: The area percentage of α-Al dendrites is ≤30%; The length of the primary dendrite arm of α-Al dendrite is ≤100 μm; The area percentage of blocky binary eutectic structure is ≤10%; The equivalent diameter of the bulk binary eutectic structure is ≤100 microns.
5. A hot-dip galvanized aluminum-magnesium coated steel sheet, characterized in that: The steel plate comprises a steel substrate and a coating attached to at least a portion of the surface of the steel substrate; the coating comprises the zinc-aluminum-magnesium alloy coating according to any one of claims 1 to 4.
6. The hot-dip galvanized aluminum-magnesium coated steel sheet according to claim 5, characterized in that: An alloy layer is contained between the zinc-aluminum-magnesium coating and the steel substrate.
7. The hot-dip galvanized aluminum-magnesium coated steel sheet according to claim 6, characterized in that: The alloy layer is composed of an Al-Fe system compound and a Mg-Si system compound.
8. A hot-dip galvanized aluminum-magnesium coated steel sheet according to claim 6 or 7, characterized in that: The average thickness of the alloy layer is 0.03 μm to 1 μm.
9. A method for preparing a hot-dip galvanized aluminum-magnesium coated steel sheet according to any one of claims 5 to 8, characterized in that: The method comprises: heating the steel substrate; Immersing the heated steel substrate into a plating solution containing the chemical components of the zinc-aluminum-magnesium alloy coating to form a coating, thereby obtaining a hot-dip zinc-aluminum-magnesium coated steel sheet; The hot-dip galvanized aluminum-magnesium coated steel sheet is cooled to below 300° C. at a set cooling rate.
10. The preparation according to claim 9, characterized in that The set cooling rate is >10K / s.
Citation Information
Patent Citations
Al-Zn-Mg-Si alloy for hot dipping steel
CN101457320A
High-corrosion-resistance hot-dip galvanized steel plate having highly uniform appearance and manufacturing method therefor
CN103620079A
Plating solution for continuous hot dipping of steel strips and dipping method thereof
CN104498850A
Hot galvanizing hot rolled steel and preparation method thereof
CN111575626A
Hot-dip zinc-aluminum-magnesium plated steel and preparation method thereof
CN115572931A
Cited By
Filamentous-corrosion-resistant hot-dip zinc-aluminum-magnesium coated steel plate and preparation method thereof
CN119663054A
Research method for influence rule of cooling speed on coating structure in hot dipping process
CN121068663A