Iridium oxide catalyst with porous structure as well as preparation method and application of iridium oxide catalyst

By using porous structure iridium oxide catalyst in PEM electrolytic hydrogen production technology, the problems of high cost and scarce resources of iridium-based catalysts are solved, and catalytic effects with high activity and stability are achieved, and the amount of iridium used in electrolytic cells is reduced. , and simplified the preparation process, suitable for industrial production.

CN119061425APending Publication Date: 2024-12-03XIAMEN ZIJIN NEW ENERGY & NEW MATERIAL TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411232108.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the existing PEM electrolytic hydrogen production technology, the use cost of iridium-based catalysts is high and the resources are scarce, making it difficult to develop low iridium oxygen evolution reaction catalysts with high activity and good stability, which limits the use of iridium in electrolytic cell equipment. .

Method used

Using a preparation method of porous structure iridium oxide catalyst, the iridium source, pore-forming ligand and initiating additive are uniformly dispersed in a mixed solution of alcohol water, and then the nanosheet cross-linked three-dimensional fluffy is formed by low-temperature evaporation and high-temperature thermal decomposition. A structured porous iridium oxide catalyst used for electrocatalytic water decomposition and anti-reverse catalyst in fuel cells.

Benefits of technology

A porous structure iridium oxide catalyst with a high specific surface area has high catalytic activity and stability, reducing the use of iridium in electrolytic cell equipment, simplifying the preparation process and suitable for industrial production, and improving the production of hydrogen by PEM electrolyzing water efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061425A_ABST
    Figure CN119061425A_ABST
Patent Text Reader

Abstract

The preparation method comprises the following steps: reacting and complexing an iridium source and a pore-forming ligand in an alcohol-water mixed solution by adopting a one-pot method, adding an oxidative initiation auxiliary agent, sequentially carrying out low-temperature evaporation and high-temperature thermal decomposition, and carrying out in-situ decomposition of gas micromolecules to generate the iridium oxide catalyst with the porous structure, a high-specific-surface-area porous structure is formed in an auxiliary manner, and the porous-structure iridium oxide catalyst is obtained. The method is simple and easy to implement, high in yield, safe and green in operation process, flexible in precursor metal iridium salt selection and beneficial to industrial production; meanwhile, the method has high expansibility, and the preparation method is provided for applying the nano-porous structure oxide to the fields of catalysis, energy, environment and the like. Meanwhile, the prepared porous-structure iridium oxide is composed of a mesoporous-microporous composite structure and has rich proton and electron conduction channels, the microstructure is of a nanosheet cross-linked three-dimensional fluffy structure, and it is facilitated that the catalyst shows high activity and stability in the water electrolysis oxygen evolution reaction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalyst materials, and in particular to a porous iridium oxide catalyst and a preparation method and application thereof. Background Art

[0002] As a zero-carbon emission energy, hydrogen energy is recognized as one of the cleanest energy sources. How to produce hydrogen at low cost, efficiently and sustainably is the primary scientific problem that humans need to solve in the future as they enter the hydrogen economy. Hydrogen production technology based on water electrolysis based on renewable energy is currently the most promising low-carbon and high-purity hydrogen production technology direction. Compared with traditional alkaline water electrolysis, proton exchange membrane water electrolysis (PEMWE) is considered to be one of the key technologies for achieving the "dual carbon" goal, especially its rapid response characteristics and excellent power grid power regulation function, which can highly match the volatility of renewable energy such as wind, light and water. Faced with the great demand for large-scale consumption of renewable energy and green hydrogen production, the international competition for PEM water electrolysis has become a hot spot. Developing catalysts with excellent activity, good stability and low cost is the key to improving the efficiency of PEM water electrolysis hydrogen production. At present, only iridium-based catalysts can maintain catalytic activity and stability for a long time in practical applications. However, due to the scarce reserves and high price of metallic iridium resources, PEM water electrolysis hydrogen production technology urgently needs to develop low-iridium oxygen evolution reaction catalysts with high activity and good stability to reduce the use of precious metal iridium in electrolyzer equipment. Summary of the invention

[0003] In view of the deficiencies in the prior art, the present invention aims to provide a porous iridium oxide catalyst and a preparation method and application thereof.

[0004] In order to achieve the above object, the present invention adopts the following technical solution:

[0005] A method for preparing a porous iridium oxide catalyst, the specific process is:

[0006] The iridium source, pore-forming ligand and initiator are uniformly dispersed and dissolved in an alcohol-water mixed solution, and after low-temperature evaporation, the precipitated crystals are subjected to high-temperature thermal decomposition to obtain a porous iridium oxide catalyst.

[0007] Furthermore, the iridium source includes one or more of chloroiridic acid, iridium trichloride, iridium tetrachloride, iridium acetylacetonate, potassium chloroiridate, sodium chloroiridate and iridium acetate.

[0008] Furthermore, the pore-forming ligand includes one or more of carbonamide, ethanolamine, dicyandiamide, melamine, thiourea and ethylenediaminetetraacetic acid.

[0009] Furthermore, the initiator aid includes one or more of sodium nitrate, potassium nitrate and lithium nitrate.

[0010] Furthermore, in the alcohol-water mixed solution, the volume ratio of ethanol to water is 0-2 but the volume of ethanol is not 0; the molar ratio of the iridium source to the pore-forming ligand is 0.01-1; and the molar ratio of the iridium source to the initiating aid is 0.001-1.

[0011] Furthermore, the temperature of the low-temperature evaporation is 50-120°C, and the temperature of the high-temperature thermal decomposition is 350-700°C.

[0012] Furthermore, the solid product obtained after the high-temperature thermal decomposition is acid-washed, washed with ultrapure water and filtered, and then low-temperature vacuum-dried at 50-80° C. to obtain a porous iridium oxide catalyst.

[0013] The present invention also provides a porous iridium oxide catalyst prepared by the above preparation method, characterized in that the microscopic morphology of the porous iridium oxide catalyst is a three-dimensional fluffy structure of cross-linked nanosheets, and the particle size is 2 to 5000 nm.

[0014] The present invention also provides an application of a porous iridium oxide catalyst prepared by the above preparation method in electrocatalytic water decomposition, wherein the porous iridium oxide catalyst is used as an anode catalyst in the electrocatalytic water decomposition.

[0015] The present invention also provides an application of a porous iridium oxide catalyst prepared by the above preparation method in a fuel cell, wherein the porous iridium oxide catalyst is used as an anti-reverse polarity catalyst in the fuel cell.

[0016] The beneficial effects of the present invention are as follows: the present invention adopts a one-pot method to react and complex the iridium source with the pore-forming ligand in an alcohol-water mixture, and adds an oxidative initiator, which is sequentially subjected to low-temperature evaporation and high-temperature thermal decomposition, and is produced by in-situ decomposition of small gas molecules, and a high specific surface area porous structure is assisted to form, thereby obtaining a porous structure iridium oxide catalyst. The preparation method of the present invention is simple and easy, with high yield, safe and green operation process, flexible selection of precursor metal iridium salt, and conducive to industrial production; at the same time, the present invention has a high degree of scalability, and provides a preparation method for nanoporous structure oxides used in catalysis, energy, environment and other fields. At the same time, the porous structure iridium oxide prepared by the present invention is composed of a mesoporous-microporous composite structure, has abundant proton and electron conduction channels, and has a microscopic morphology of a three-dimensional fluffy structure of cross-linked nanosheets, which is conducive to promoting the catalyst to exhibit high activity and stability in the electrolytic water oxygen evolution reaction. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a SEM image of the porous iridium oxide catalyst prepared in Example 1 of the present invention;

[0018] Figure 2TEM image of the porous iridium oxide catalyst prepared in Example 1 of the present invention;

[0019] Figure 3 The BET diagram of the porous iridium oxide catalyst prepared in Example 1 of the present invention;

[0020] Figure 4 This is a polarization curve diagram of electrochemical oxygen evolution of the porous iridium oxide catalyst prepared in Example 1 of the present invention;

[0021] Figure 5 This is a performance diagram of the iridium oxide catalyst prepared in Example 1 of the present invention for use in a PEM water electrolysis membrane electrode device;

[0022] Figure 6 This is a SEM image of the porous iridium oxide catalyst prepared in Example 2 of the present invention;

[0023] Figure 7 This is a polarization curve diagram of electrochemical oxygen evolution of the porous iridium oxide catalyst prepared in Example 2 of the present invention;

[0024] Figure 8 This is a polarization curve diagram of electrochemical oxygen evolution of the porous iridium oxide catalyst prepared in Example 3 of the present invention;

[0025] Fig. 9 This is the SEM image of the porous iridium oxide catalyst prepared in Comparative Example 1. DETAILED DESCRIPTION

[0026] The present invention will be further described below in conjunction with the accompanying drawings. It should be noted that this embodiment is based on the technical solution and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to this embodiment.

[0027] Example 1

[0028] This embodiment provides a method for preparing a porous iridium oxide catalyst, and the specific process is as follows:

[0029] 1) The iridium source chloroiridic acid and the pore-forming ligand carbonamide are mixed at a molar ratio of 1:10, and then the initiator auxiliary sodium nitrate is added and continued to mix, and the molar ratio of sodium nitrate to chloroiridic acid is 50:1. Then 25 mL of ethanol and 25 mL of ultrapure water are added in sequence, and stirred and mixed at room temperature to obtain a precursor mixture after dissolution.

[0030] 2) placing the precursor mixture obtained in step 1) in an 80° C. oil bath for heating and evaporation, and after crystallization and drying, grinding the product and placing it in a 450° C. heating furnace for high-temperature thermal decomposition.

[0031] 3) The solid product obtained by high-temperature thermal decomposition in step 2) is soaked in a 1 mol / L sulfuric acid solution for 10 hours, then washed and filtered with ultrapure water, and when the ion conductivity in the filtrate is <5S / cm, the product is collected and vacuum dried at 60°C to obtain a porous iridium oxide catalyst. The catalyst is dried and stored at room temperature.

[0032] The synthesized porous structure iridium oxide catalyst was characterized and tested. Figure 1 This is the scanning electron microscope (SEM) image of the catalyst, from which it can be seen that the morphology of the catalyst is a three-dimensional fluffy stacking structure of cross-linked and self-assembled nanosheets. Figure 2 The TEM image of the iridium oxide catalyst shows that the catalyst has a large number of micropores and mesoporous structures (indicated by the small circles in the image), and there are obvious iridium dioxide (101) interplanar spacing stripes, indicating that the catalyst has a good micro-mesoporous composite morphology and crystal structure. The obtained iridium oxide catalyst was further subjected to the BET test of specific surface area, as shown in FIG. Figure 3 The results of nitrogen adsorption and desorption tests further showed that the catalyst has a porous adsorption structure with coexistence of micro / mesopores, and its specific surface area is as high as 277.8m 2 g -1 .

[0033] Electrocatalytic oxygen evolution reaction (OER) test

[0034] The prepared porous iridium oxide catalyst was used for oxygen evolution reaction test in an acidic environment. A three-electrode test system was used. The working electrode was a rotating disk electrode, the counter electrode was a carbon rod, and the reference electrode was a standard hydrogen electrode. 4 mg of the catalyst was weighed and dispersed in an aqueous solution of isopropanol (190 μL of water, 300 μL of isopropanol). After ultrasonic dispersion for 30 minutes, 10 μL of Nafion solution was added. After further mixing and ultrasonic dispersion, the catalyst slurry ink was obtained. Take 5 μL of the prepared slurry ink and evenly drop it on a glassy carbon electrode with a diameter of 5 mm. The loading capacity is 0.2 mg cm-2. After evaporation and drying at room temperature, test it. Select 0.1 mol / L perchloric acid solution as the test electrolyte, and use linear sweep voltammetry to test the electrochemical data with a scan rate of 2 mV / s. The test results are as follows Figure 4 As shown, at 10 mA cm -2 At a current density of , the overpotential of the porous iridium oxide catalyst is 241 mV, which is much lower than the overpotential of common commercial iridium oxide (about 300 mV).

[0035] Membrane electrode preparation and testing

[0036] The prepared porous iridium oxide catalyst is used in a proton exchange membrane (PEM) water electrolysis device as a catalyst for oxygen evolution reaction on the anode side of the membrane electrode, and a commercial platinum carbon catalyst is used as a catalyst for hydrogen evolution reaction on the cathode side. The catalysts of the cathode and cathode are sprayed on both sides of the proton exchange membrane through the preparation method of catalyst coated membrane (CCM), and then assembled into a PEM device with a gas diffusion layer, bipolar plate, sealing ring, etc. after being made into a membrane electrode. The test results are as follows Figure 5 As shown, the iridium loading at the anode is only 0.626 mg cm -2 When 2A cm -2 Under the current density, the electrolysis potential is only 1.789V, indicating that the catalyst has good membrane electrode device performance.

[0037] In summary, the porous iridium oxide catalyst prepared in this embodiment can be well adapted to the OER catalyst in an acidic environment, and its intrinsic electrocatalytic activity and membrane electrode device performance are excellent, showing great application potential in PEM water electrolysis devices.

[0038] Example 2

[0039] This embodiment provides a method for preparing a porous iridium oxide catalyst, and the specific process is as follows:

[0040] The iridium source chloroiridic acid and the pore-forming ligand carbonamide are mixed in a molar ratio of 1:20, and then the initiator sodium nitrate is added to continue mixing, and the molar ratio of sodium nitrate to chloroiridic acid is 100:1. Then 30mL of ethanol and 30mL of ultrapure water are added in turn, stirred and mixed at room temperature, and a precursor mixture is obtained after dissolution. The obtained precursor mixture is placed in an 80°C oil bath pot, heated and evaporated, and after crystallization and drying, the product is ground and placed in a 450°C heating furnace for high-temperature thermal decomposition. The solid product obtained by high-temperature thermal decomposition is acid-washed and soaked with a 1mol / L perchloric acid solution, then washed and filtered with ultrapure water. When the ionic conductivity in the filtrate is <5S / cm, the product is collected and vacuum dried at 60°C to obtain a porous structure iridium oxide catalyst. Dry and store at room temperature. The synthesized porous structure iridium oxide catalyst is characterized and tested. Figure 6 This is a scanning electron microscope (SEM) image of the catalyst prepared in this example. It can be seen from the image that the catalyst is a fluffy three-dimensional stacking structure of self-assembled thin nanosheets. Figure 7 The electrochemical performance test diagram of the catalyst prepared in this example is shown in Figure 1. -2 At a current density of , the overpotential of the porous iridium oxide catalyst is 248 mV.

[0041] Example 3

[0042] This embodiment provides a method for preparing a porous iridium oxide catalyst, and the specific process is as follows:

[0043] The iridium source iridium tetrachloride and the pore-forming ligand ethanolamine are mixed in a molar ratio of 1:10, and then the initiator sodium nitrate is added and continued to mix, and the molar ratio of sodium nitrate to iridium tetrachloride is 70:1. Then 20mL of ethanol and 10mL of ultrapure water are added in turn, stirred and mixed at room temperature, and a precursor mixture is obtained after dissolution. The obtained precursor mixture is placed in an 80°C oil bath pot, heated and evaporated, and after crystallization and drying, the product is ground and placed in a 500°C heating furnace for high-temperature thermal decomposition. The solid product obtained by high-temperature thermal decomposition is acid-washed and soaked with a 1mol / L sulfuric acid solution, then washed and filtered. When the ionic conductivity in the filtrate is <5S / cm, the product is collected and vacuum dried at 60°C to obtain a porous structure iridium oxide catalyst. Dry and store at room temperature.

[0044] The synthesized porous iridium oxide catalyst was characterized and its performance tested. Figure 8 The electrochemical performance test diagram of the catalyst is shown in Figure 1. -2 At a current density of , the overpotential of the porous iridium oxide catalyst is 294 mV.

[0045] Example 4

[0046] This embodiment provides a method for preparing a porous iridium oxide catalyst, and the specific process is as follows:

[0047] The iridium source iridium tetrachloride and the pore-forming ligand ethanolamine are mixed in a molar ratio of 1:10, and then the initiator auxiliary sodium nitrate is added to continue mixing, and the molar ratio of sodium nitrate to iridium tetrachloride is 70:1. Then add 20mL of ethanol and 10mL of ultrapure water in turn, stir and mix at room temperature, and obtain a precursor mixture after dissolution. The obtained precursor mixture is placed in a 50°C vacuum rotary evaporator for heating. After the rotary evaporator is crystallized and dried, the product is ground and placed in a 700°C heating furnace for high-temperature thermal decomposition. The solid product obtained by high-temperature thermal decomposition is acid-washed and soaked with 1mol / L sulfuric acid solution, then washed and filtered. When the ionic conductivity in the filtrate is <5S / cm, the product is collected and vacuum-dried at 80°C to obtain a porous structure iridium oxide catalyst. Dry and store at room temperature. The porous structure iridium oxide catalyst synthesized and prepared by the method of this embodiment is characterized and performance tested. The electrochemical performance test shows that the catalyst is 10mA cm -2 The catalytic overpotential is 300 mV at a current density of .

[0048] Comparative Example 1

[0049] The iridium source chloroiridic acid and the pore-forming ligand carbonamide are mixed in a molar ratio of 1:10, and then the initiator sodium nitrate is added and continued to mix, and the molar ratio of sodium nitrate to chloroiridic acid is 50:1. Then add 25mL of ethanol and 25mL of ultrapure water in turn, stir and mix at room temperature, and obtain a precursor mixture after dissolution. The obtained precursor mixture is placed in an 80℃ oil bath pot, heated and evaporated, and after crystallization and drying, the product is ground and placed in a 700℃ heating furnace for high-temperature thermal decomposition. The product obtained by high-temperature thermal decomposition is acid-washed and soaked with 1mol / L sulfuric acid solution, then washed and filtered. When the ionic conductivity in the filtrate is <5S / cm, the product is collected and vacuum dried at 60℃ to obtain a porous structure iridium oxide catalyst. Dry and store at room temperature.

[0050] The porous iridium oxide catalyst synthesized and prepared in this comparative example was subjected to characterization tests. Fig. 9 This is the SEM image of the catalyst, from which it can be seen that too high a thermal decomposition temperature will cause the catalyst nanosheets to become thicker and thicker, and the particle size to increase, resulting in a decrease in catalyst performance.

[0051] For those skilled in the art, various corresponding changes and modifications can be made according to the above technical solutions and concepts, and all of these changes and modifications should be included in the protection scope of the claims of the present invention.

Claims

1. A method for preparing a porous iridium oxide catalyst, characterized in that: The specific process is: The iridium source, pore-forming ligand and initiator are uniformly dispersed and dissolved in an alcohol-water mixed solution, and after low-temperature evaporation, the precipitated crystals are subjected to high-temperature thermal decomposition to obtain a porous iridium oxide catalyst.

2. The preparation method according to claim 1, characterized in that: The iridium source includes one or more of chloroiridic acid, iridium trichloride, iridium tetrachloride, iridium acetylacetonate, potassium chloroiridate, sodium chloroiridate and iridium acetate.

3. The preparation method according to claim 1, characterized in that: The pore-forming ligand includes one or more of carbonamide, ethanolamine, dicyandiamide, melamine, thiourea and ethylenediaminetetraacetic acid.

4. The preparation method according to claim 1, characterized in that: The initiator aid includes one or more of sodium nitrate, potassium nitrate and lithium nitrate.

5. The preparation method according to claim 1, characterized in that: In the alcohol-water mixed solution, the volume ratio of ethanol to water is 0-2, but the volume of ethanol is not 0; the molar ratio of the iridium source to the pore-forming ligand is 0.01-1; and the molar ratio of the iridium source to the initiating auxiliary agent is 0.001-1.

6. The preparation method according to claim 1, characterized in that: The temperature of the low-temperature evaporation is 50-120°C, and the temperature of the high-temperature thermal decomposition is 350-700°C.

7. The preparation method according to claim 1, characterized in that: The solid product obtained after high-temperature thermal decomposition is acid-washed, washed with ultrapure water and filtered, and then low-temperature vacuum-dried at 50-80° C. to obtain a porous iridium oxide catalyst.

8. A porous iridium oxide catalyst prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The microscopic morphology of the porous iridium oxide catalyst is a three-dimensional fluffy structure of cross-linked nanosheets, and the particle size is 2 to 5000 nm.

9. Use of a porous iridium oxide catalyst prepared by the preparation method according to any one of claims 1 to 7 in electrocatalytic water decomposition, characterized in that: The porous iridium oxide catalyst is used as an anode catalyst in electrocatalytic water decomposition.

10. Use of a porous iridium oxide catalyst prepared by the preparation method according to any one of claims 1 to 7 in a fuel cell, characterized in that: The porous iridium oxide catalyst is used as an anti-reverse polarity catalyst in a fuel cell.

Citation Information

Cited By

  • Iridium oxide catalyst with dendritic pore structure, preparation method and application of iridium oxide catalyst in proton exchange membrane water electrolysis technology

    CN119706982A