Preparation method of nitrogen-doped carbon fiber loaded Ni-MoC nanoparticles for electro-catalytic hydrogen evolution in full pH range
Through the preparation method of nitrogen-doped carbon fiber-supported Ni-MoC nanoparticles, the high cost of precious metal catalysts and the agglomeration of molybdenum carbide is solved, and the electrocatalytic hydrogen evolution performance with high activity and long-term stability is achieved, and the catalyst in the prior art is overcome. Issues of stability and cost.
Patent Information
- Application Number
- CN202411278886.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-12-03
AI Technical Summary
In the existing electrocatalytic hydrogen production technology, precious metal catalysts are costly and molybdenum carbide materials are prone to agglomeration during high-temperature calcination, resulting in reduced exposure to active sites and reduced catalyst stability, making it difficult to develop low-cost, high-activity and long-term stability. Non-precious metal catalyst.
The preparation method of nitrogen-doped carbon fiber-supported Ni-MoC nanoparticles is adopted. By combining electrospinning and high-temperature carbonization, the agglomeration of Ni and MoC nanoparticles is avoided, the MoC electronic structure is adjusted, and the activity and stability of the catalyst are improved.
High catalytic activity and long-term stability in the full pH range are achieved, catalyst costs are reduced, active site exposure is avoided due to agglomeration is reduced, and specific surface area and electrocatalytic hydrogen evolution performance are improved.
Smart Images

Figure CN119061427A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a nano material capable of performing an electrocatalytic hydrogen evolution reaction in a full pH range, and belongs to the technical field of electrocatalytic water decomposition and hydrogen production. Background Art
[0002] Hydrogen energy is considered to be an ideal energy carrier to replace fossil energy due to its advantages such as cleanliness, renewable energy and high energy density.
[0003] Since it was first discovered in the 18th century, the technology of producing hydrogen by electrolysis of water has experienced many qualitative leaps from early experiments to modern applications. Today, this technology plays an increasingly important role in energy transformation and sustainable development. As a key component in the hydrogen production process, catalysts can effectively reduce the energy consumption of water electrolysis. Pt / C catalysts are currently commercial catalysts for hydrogen production due to their high intrinsic activity. However, the scarce reserves of precious metals have greatly increased the cost of catalysts, which has become a bottleneck problem in the current electrocatalytic hydrogen production technology. Therefore, the development of low-cost, highly active and long-term stable non-precious metal-based catalysts is the key to the development of water electrolysis hydrogen production technology.
[0004] Metallic Ni and precious metal Pt belong to the same group of elements with similar chemical properties. Metallic Ni has good acid and alkali corrosion resistance, high conductivity and good ductility, so it plays an important role in the field of electrocatalytic hydrogen production. Transition metal carbides, such as molybdenum carbide, tungsten carbide and vanadium carbide, are considered to be ideal materials to replace precious metal catalysts due to their platinum-like electronic structure. Among them, molybdenum carbide exhibits excellent hydrogen evolution activity and stability over the entire pH range. However, the material requires high-temperature calcination during the preparation process, which inevitably leads to particle agglomeration, greatly reducing the number of exposed active sites and catalyst stability. Therefore, it is urgent to develop a simple method that can effectively inhibit the agglomeration of molybdenum carbide, so as to prepare a catalyst with high catalytic activity and long-term stability. Summary of the invention
[0005] Based on the above-mentioned background technical problems, the purpose of the present invention is to provide a method for preparing Ni-MoC nanoparticles supported by nitrogen-doped carbon fibers. The material has the following excellent characteristics: the synergistic effect between Ni and MoC helps the adsorption and desorption of hydrogen intermediates on the catalyst surface, thereby enhancing the hydrogen evolution activity of the hybrid material. The hierarchical porous structure of nitrogen-doped carbon fibers can not only promote the full contact between the electrolyte and the catalyst, but also improve the stability of the catalyst.
[0006] The above purpose is achieved through the following technical solutions:
[0007] A method for preparing nitrogen-doped carbon fiber-supported Ni-MoC nanoparticles for electrocatalytic hydrogen evolution over a full pH range, specifically comprising the following steps:
[0008] (1) Nickel nitrate hexahydrate and 2-methylimidazole are dissolved in methanol respectively; the methanol solutions of nickel nitrate hexahydrate and 2-methylimidazole are mixed, stirred magnetically, and the product is collected by centrifugation. The obtained precipitate is washed with anhydrous ethanol and dried to obtain Ni-ZIF
[0009] (2) Add polyacrylonitrile to N,N-dimethylformamide and stir until a clear solution is obtained. Add molybdenum acetylacetonate and the Ni-ZIF prepared in step (1) to the solution, stir magnetically to obtain a spinning solution, and then obtain a spinning membrane by electrospinning.
[0010] (3) The electrospun membrane obtained in step (2) is pre-oxidized in a muffle furnace.
[0011] (4) The product after pre-oxidation in step (3) is calcined in an argon atmosphere to obtain the final product.
[0012] Preferably, in step (1) of the present invention, the masses of nickel nitrate hexahydrate and dimethylimidazole are 1 g and 4 g respectively; and the required volumes of methanol are 100 mL and 50 mL respectively.
[0013] Preferably, in step (1) of the present invention, the magnetic stirring time is 24 h and the temperature is room temperature.
[0014] Preferably, in step (2) of the present invention, the mass of polyacrylonitrile is 0.7 g, the volume of N,N-dimethylformamide is 8 mL, and the magnetic stirring time is 4 h.
[0015] Preferably, in step (2) of the present invention, the mass of Ni-ZIF added is 0.3 g, the mass of molybdenum acetylacetonate oxide is 0.2 g, and stirring is performed at room temperature for 12 h.
[0016] Preferably, in step (2) of the present invention, the spinning solution is injected into a 10 mL syringe, the distance between the syringe and the collector is 15 cm, the applied voltage is 15 kV, and the pushing speed is 0.1 mm min –1 .
[0017] Preferably, the pre-oxidation temperature in step (3) of the present invention is 250 o C, the heating rate is 1 o C min –1 , the pre-oxidation time was 2 h.
[0018] Preferably, in step (4) of the present invention, the carbonization conditions are first at 550 o C for 1 h, and then heated to 900 o C for 2 h, with a heating rate of 5 o C min –1 .
[0019] Technical effect: Compared with the prior art, the outstanding effects of the present invention are:
[0020] (1) The present invention adopts a method combining electrospinning and high-temperature carbonization, introduces Ni-ZIF as a precursor, and in situ grows Ni-MoC nanoparticles on nitrogen-doped carbon fibers. Nitrogen-doped carbon fibers can not only effectively avoid the agglomeration of Ni and MoC nanoparticles, thereby exposing more active sites, but also greatly improve the stability of the catalyst. The introduction of Ni can effectively adjust the electronic structure of MoC, making the catalyst exhibit higher catalytic activity.
[0021] (2) The preparation method adopted by the present invention has the advantages of cheap raw materials, easy repetition, and simple process. In addition, compared with molybdenum carbide prepared from a gaseous carbon source, molybdenum carbide prepared using carbon fiber as a solid carbon source can control the degree of carbonization, effectively avoid excessive carbonization or incomplete carbonization, and fully expose the active sites. The electrocatalyst prepared by the present invention has a larger specific surface area and excellent electrocatalytic hydrogen evolution performance.
[0022] (3) The catalyst prepared by the present invention is a self-supporting material, which overcomes the disadvantage that a binder needs to be added when a powdered catalyst is prepared into a working electrode. It not only improves the conductivity and mass transfer capacity, but also greatly improves the long-term stability of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Shown is the X-ray diffraction pattern of the catalyst prepared in Example 1 of the present invention.
[0025] Figure 2 Shown is a scanning electron microscope image of the catalyst prepared in Example 1 of the present invention.
[0026] Figure 3 Shown is a transmission electron microscope image of the catalyst prepared in Example 1 of the present invention.
[0027] Figure 4 Shown are the high-angle annular dark field scanning transmission electron microscopy images (HAADF-STEM) and element distribution maps of the catalyst prepared in Example 1 of the present invention, wherein a is the STEM image, and bf are element distribution maps of different elements.
[0028] Figure 5Shown is the nitrogen adsorption-desorption isotherm of the catalyst prepared in Example 1 of the present invention.
[0029] Figure 6 Shown is the pore size distribution diagram of the catalyst prepared in Example 1 of the present invention.
[0030] Figure 7 Shown is the linear sweep voltammetry (LSV) curve of the electrocatalytic hydrogen evolution reaction of the catalyst prepared in Example 1 of the present invention in 1 M KOH, 0.5 M H2SO4 and 1 M PBS electrolyte. DETAILED DESCRIPTION
[0031] Now, various exemplary embodiments of the present invention are described in conjunction with specific examples. It should be noted that, for those skilled in the art, several improvements can be made without departing from the concept of the present invention, and all of these belong to the protection scope of the present invention. Example 1
[0032] A method for preparing nitrogen-doped carbon fiber-loaded Ni-MoC nanoparticles comprises the following steps:
[0033] Step 1: Dissolve 1 g nickel nitrate hexahydrate and 4 g 2-methylimidazole in 100 mL and 50 mL methanol, respectively. Then, mix the above solutions and stir at room temperature for 24 h. After the reaction, collect the product by centrifugation (centrifugal speed is 8000 rpm, centrifugal time is 5 min), wash the yellow-green precipitate with anhydrous ethanol several times, and dry it in vacuum at 60 °C for 12 h to obtain Ni-ZIF.
[0034] Step 2: Add 0.7 g of polyacrylonitrile to 8 mL of N,N-dimethylformamide and stir for 4 h to obtain a clear solution. Then, add 0.2 g of molybdenum acetylacetonate oxide and 0.3 g of prepared Ni-ZIF to the above solution and stir at room temperature for 12 h to obtain a spinning solution; inject the spinning solution into a 10 mL syringe, the distance between the syringe and the collector is 15 cm, the applied voltage is 15 kV, and the push speed is 0.1 mm min –1 , and the nanofiber membrane was collected on tin foil.
[0035] Step 3: The obtained nanofiber membrane was heated in a muffle furnace at 250 °C for 1 °C min –1 The pre-oxidation was carried out at a heating rate of 2 h.
[0036] Step 4: The pre-oxidized fiber membrane was calcined at 550 °C for 1 h in an argon atmosphere and then heated to 900 °C for 2 h. Example 2
[0037] A method for preparing nitrogen-doped carbon fiber-loaded Ni-MoC nanoparticles comprises the following steps:
[0038] Step 1: Dissolve 1 g nickel nitrate hexahydrate and 4 g 2-methylimidazole in 100 mL and 50 mL methanol, respectively. Then mix the above solutions and stir at room temperature for 24 h. After the reaction is completed, collect the product by centrifugation (centrifugal speed is 8000 rpm, centrifugal time is 5 min), wash the obtained yellow-green precipitate with anhydrous ethanol several times, and then dry it in a vacuum drying oven at 60 ° C for 12 h to obtain Ni-ZIF.
[0039] Step 2: 0.7 g of polyacrylonitrile was added to 8 mL of N,N-dimethylformamide and stirred for 4 h to obtain a clear solution. Then, 0.3 g of molybdenum acetylacetonate oxide and 0.2 g of prepared Ni-ZIF were added to the above solution and stirred at room temperature for 12 h to obtain a spinning solution. The spinning solution was injected into a 10 mL syringe with a distance of 15 cm between the syringe and the collector, an applied voltage of 15 kV, and a push speed of 0.1 mm min –1 , and the nanofiber membrane was collected on tin foil.
[0040] Step 3: The obtained nanofiber membrane was heated in a muffle furnace at 250 °C for 1 °C min –1 The heating rate was 2 h for pre-oxidation.
[0041] Step 4: The pre-oxidized fiber membrane was calcined at 550 °C for 1 h in an argon atmosphere and then heated to 900 °C for 2 h. Example 3
[0042] Step 1: Dissolve 1 g nickel nitrate hexahydrate and 4 g 2-methylimidazole in 100 mL and 50 mL methanol, respectively. Then mix the above solutions and stir at room temperature for 24 h. After the reaction is completed, collect the product by centrifugation (centrifugal speed is 8000 rpm, centrifugal time is 5 min), wash the obtained yellow-green precipitate with anhydrous ethanol several times, and then dry it in a vacuum drying oven at 60 ° C for 12 h to obtain Ni-ZIF.
[0043] Step 2: 0.7 g of polyacrylonitrile was added to 8 mL of N,N-dimethylformamide and stirred for 4 h to obtain a clear solution. Then, 0.1 g of molybdenum acetylacetonate oxide and 0.4 g of prepared Ni-ZIF were added to the above solution and stirred at room temperature for 12 h to obtain a spinning solution. The spinning solution was injected into a 10 mL syringe with a distance of 15 cm between the syringe and the collector, an applied voltage of 15 kV, and a push speed of 0.1 mm min –1 , and the nanofiber membrane was collected on tin foil.
[0044] Step 3: The obtained nanofiber membrane was heated in a muffle furnace at 250 °C for 1 °C min –1 The heating rate was 2 h for pre-oxidation.
[0045] Step 4: The pre-oxidized fiber membrane was calcined at 550 °C for 1 h in an argon atmosphere and then heated to 900 °C for 2 h. Comparative Example 1
[0046] Compared with Example 1, the only difference is that acetylacetonate molybdenum oxide is not added, the mass of Ni-ZIF added to the spinning solution is 0.5 g, and the obtained material is a hybrid material of nitrogen-doped carbon fiber loaded with metal Ni nanoparticles. Comparative Example 2
[0047] Compared with Example 1, the only difference is that Ni-ZIF is not added, the mass of acetylacetonate molybdenum oxide added to the spinning solution is 0.5 g, and the obtained material is a hybrid material of nitrogen-doped carbon fiber loaded with MoC nanoparticles. Performance Testing
[0048] The electrocatalytic hydrogen evolution performance of the nitrogen-doped carbon fiber-supported Ni-MoC nanoparticles prepared in this example was tested as follows: All electrochemical measurements were performed on a CHI 760E electrochemical workstation. Ag / AgCl was used as the reference electrode in acidic or neutral media, and Hg / HgO was used as the reference electrode in alkaline media. A graphite rod was used as the counter electrode. The prepared catalyst was directly cut into a 1 cm × 1 cm self-supporting material as a working electrode.
[0049] The performance test results of Examples 1-3 and Comparative Examples 1-2 are recorded in Table 1.
[0050] Table 1 Performance test results of Examples 1 to 3 and Comparative Examples 1 to 2 Overpotential A (mV) Overpotential B (mV) Overpotential C (mV) Example 1 108 138 192 Example 2 137 144 239 Example 3 140 155 265 Comparative Example 1 202 192 268 Comparative Example 2 230 220 300
[0051] A, B, and C represent the test conditions of 1 M KOH, 0.5 M H2SO4, and 1 M PBS, respectively. The measured overpotential is 10 mA cm –2 The value of current density.
Claims
1. A method for preparing nitrogen-doped carbon fiber-supported Ni-MoC nanoparticles for electrocatalytic hydrogen evolution over a full pH range, Features , the steps are as follows: (1) Nickel nitrate hexahydrate and 2-methylimidazole were dissolved in methanol respectively, and then the above solutions were mixed and stirred, and the products were collected by centrifugation. The obtained yellow-green precipitate was washed several times with anhydrous ethanol and then dried to obtain a Ni-ZIF precursor; (2) Add polyacrylonitrile to N,N-dimethylformamide and stir until a clear solution is obtained; Adding Ni-ZIF and molybdenum acetylacetonate to the above solution, stirring continuously to obtain a spinning solution, injecting the spinning solution into a syringe, preparing nanofibers by electrospinning, and collecting on tin foil to obtain a nanofiber membrane; (3) pre-oxidizing the obtained nanofiber membrane in an air atmosphere; (4) The pre-oxidized fiber membrane is carbonized in a carrier gas atmosphere to obtain the hybrid material of the nitrogen-doped carbon fiber loaded with Ni-MoC nanoparticles.
2. The method for preparing nitrogen-doped carbon fiber-supported Ni-MoC nanoparticles for electrocatalytic hydrogen evolution over a full pH range according to claim 1, Features: In the step (1), the masses of nickel nitrate hexahydrate and 2-methylimidazole are 1 g and 4 g, respectively; the volumes of methanol required are 100 mL and 50 mL, respectively; the magnetic stirring time is 24 h, and the stirring is carried out at room temperature.
3. The preparation method according to claim 1, Features: In step (2), the mass of polyacrylonitrile is 0.7 g, the volume of N,N-dimethylformamide is 8 mL, and the stirring time is 4 h.
4. The preparation method according to claim 1, Features: The mass of Ni-ZIF added in step (2) is 0.3 g, the mass of molybdenum acetylacetonate oxide is 0.2 g, and the stirring time is 12 h.
5. The preparation method according to claim 1, Features: In step (2), the spinning solution is injected into a 10 mL syringe, the distance between the syringe and the collector is 15 cm, the applied voltage is 15 kV, and the pushing speed is 0.1 mm min –1 .
6. The preparation method according to claim 1, Features: The pre-oxidation temperature in step (3) is 250 o C, the heating rate is 1 o C min –1 , the pre-oxidation time was 2 h.
7. The preparation method according to claim 1, Features: In step (4), the carbonization conditions are firstly at 550 o C for 1 h, then heated to 900 o C for 2 h, with a heating rate of 5 o C min –1 The carrier gas was argon with a flow rate of 2-10 mL min –1 .
8. The nitrogen-doped carbon fiber loaded Ni-MoC nanoparticle hybrid material obtained by the preparation method according to any one of claims 1 to 7, Features The material appears as nanofibers with a rough surface.
9. The nitrogen-doped carbon fiber-supported Ni-MoC nanoparticle hybrid material according to claim 8 is suitable for electrocatalytic hydrogen evolution over a full pH range.
Citation Information
Cited By
Bamboo-like carbon nanofiber loaded with nickel-cobalt alloy and preparation method and application of bamboo-like carbon nanofiber
CN119710789A