Novel cyanide-free zinc plating electroplating liquid formula

The novel cyanide-free zinc plating solution, using p-methoxybenzaldehyde as a brightener, addresses stability and compatibility issues, resulting in stable and bright coatings with reduced environmental impact and lower maintenance costs.

CN119061443APending Publication Date: 2024-12-03FOSHAN RENCHANG TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411028266.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Current cyanide-free zinc plating processes face issues with stability, compatibility, coating quality, corrosion, formulation complexity, current efficiency, and cost, which hinder their widespread application.

Method used

A novel cyanide-free zinc plating solution incorporating p-methoxybenzaldehyde as a brightener, along with other components, enhances compatibility and stability, improving coating brightness and uniformity.

Benefits of technology

The solution achieves stable, bright, and uniform zinc coatings with reduced environmental impact, extending the solution's service life and lowering maintenance costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004969746620000011
    Figure BDA0004969746620000011
  • Figure BDA0004969746620000021
    Figure BDA0004969746620000021
  • Figure BDA0004969746620000061
    Figure BDA0004969746620000061
Patent Text Reader

Abstract

The invention discloses a formula of a novel cyanide-free zinc plating electroplating solution. The formula of the novel cyanide-free zinc plating electroplating solution comprises the following components: a complexing agent, a leveling agent, a brightening agent, a wetting agent, an antioxidant and an auxiliary additive, the brightener is selected from at least one of benzalacetone, benzylamine, acetylene alcohol compounds, benzyl chloride, thiourea and derivatives thereof, and p-methoxybenzaldehyde. According to the formula of the novel cyanide-free zinc plating electroplating solution disclosed by the invention, by adding the methoxybenzaldehyde brightener, the compatibility and the stability of all components of the cyanide-free zinc plating electroplating solution can be effectively achieved, and therefore the problem that an existing cyanide-free zinc plating electroplating solution is poor in compatibility, and poor chemical reactions or precipitates are generated is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a novel cyanide-free zinc plating solution formula, belonging to the technical field of cyanide-free zinc plating. Background Art

[0002] Traditional zinc plating processes often use cyanide as a key component of the electroplating solution, but cyanide has extremely high toxicity and environmental hazards, which limits its application. Therefore, the cyanide-free zinc plating process has gradually become the focus of research and application. However, the current cyanide-free zinc plating process still has some shortcomings in terms of brightness and coating uniformity, which needs further improvement and optimization.

[0003] Although cyanide-free electroplating solutions have significant advantages in terms of environmental friendliness and operational safety, they still face challenges in terms of stability, coating quality, corrosion issues, formulation complexity, current efficiency and cost. In order to achieve the widespread application of cyanide-free electroplating technology, continuous research and improvement in chemical formulation is needed to overcome these problems and improve the overall performance of cyanide-free electroplating. Summary of the invention

[0004] The purpose of the present application is to provide a novel cyanide-free zinc plating solution formula. Adding p-methoxybenzaldehyde brightener into the formula can effectively solve the compatibility between the components in the cyanide-free zinc plating solution, thereby solving the technical problems of the existing cyanide-free zinc plating solution being unstable, poorly compatible, and producing undesirable chemical reactions or precipitation.

[0005] According to one aspect of the present application, a novel cyanide-free zinc plating solution formula is provided, wherein the novel cyanide-free zinc plating solution formula comprises the following components in parts by weight:

[0006]

[0007] The brightener is selected from at least one of benzalkyne acetone, benzylamine, acetylene alcohol compounds, benzyl chloride, thiourea and its derivatives, and p-methoxybenzaldehyde.

[0008] Optionally, the brightener is p-methoxybenzaldehyde.

[0009] Optionally, the acetylene alcohol compound is selected from at least one of acetylene methanol, 1-ethynyl cyclohexanol and propargyl alcohol.

[0010] Optionally, the complexing agent is selected from at least one of ethylenediaminetetraacetic acid, sodium citrate, triethanolamine and glycine.

[0011] Optionally, the leveling agent is selected from at least one of polyethylene glycol, polyacrylamide, and sodium N,N-dimethyldithiocarbamate.

[0012] Optionally, the wetting agent is selected from sodium alkyl sulfonate and / or sodium alkylbenzene sulfonate.

[0013] Optionally, the antioxidant is selected from ascorbic acid and / or sodium metabisulfite.

[0014] Optionally, the auxiliary additive is selected from at least one of aluminum salt, zinc salt, potassium salt, ammonium salt and pH regulator.

[0015] Optionally, the aluminum salt is at least one of aluminum chloride, aluminum sulfate, and aluminum nitrate.

[0016] Optionally, the zinc salt is selected from at least one of zinc chloride, zinc sulfate and zinc nitrate.

[0017] Optionally, the potassium salt is selected from at least one of potassium chloride, potassium sulfate and potassium nitrate.

[0018] Optionally, the ammonium salt is selected from at least one of ammonium chloride, ammonium nitrate and ammonium sulfate.

[0019] Optionally, the pH adjuster is selected from at least one of boric acid, acetic acid, sodium hydroxide and potassium hydroxide.

[0020] As an optional implementation method, the present application is implemented through the following technical solutions:

[0021] The present application provides a novel pentacyanogen zinc plating solution formula, comprising the following components:

[0022]

[0023] The leveling agent is polyethylene glycol, and the dosage is 0.1-0.5 g / L, which can be adjusted according to needs.

[0024] Compared with other brighteners, p-methoxybenzaldehyde has a specific chemical structure, in which the methoxy group can provide a unique brightening effect. This structure may show different physical and chemical properties during the electroplating process; it improves the brightness and aesthetics of the coating. During electroplating, it helps to reduce defects on the surface of the coating, increase reflectivity, and make the coating surface smoother and more shiny. In addition, p-methoxybenzaldehyde is a natural compound, and using it as part of the cyanide-free zinc plating solution can reduce the impact on the environment. p-methoxybenzaldehyde helps to improve the stability of the electroplating solution and reduce the decomposition and deterioration of the plating solution during use, which helps to extend the service life of the electroplating solution and further reduce maintenance costs.

[0025] The beneficial effects of this application include:

[0026] 1) The novel cyanide-free zinc plating solution formula provided in the present application, by adding p-methoxybenzaldehyde brightener into the formula, can effectively solve the compatibility between the components in the cyanide-free zinc plating solution, thereby solving the technical problems of the existing cyanide-free zinc plating solution being unstable, having poor compatibility, and producing undesirable chemical reactions or precipitation.

[0027] 2) The novel cyanide-free zinc plating solution provided in the present application has a p-methoxybenzaldehyde brightener added therein. P-methoxybenzaldehyde is a natural compound, and using it as part of the cyanide-free zinc plating solution can reduce the impact on the environment. P-methoxybenzaldehyde helps to improve the stability of the plating solution and reduce the decomposition and deterioration of the plating solution during use, which helps to extend the service life of the plating solution and further reduce maintenance costs. DETAILED DESCRIPTION

[0028] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0029] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.

[0030] Unless otherwise specified, the instruments used in this application are conventional existing instruments and equipment and operating conditions.

[0031] Example 1

[0032] Prepare one liter of plating solution by weighing 2 g of ethylenediaminetetraacetic acid complexing agent, 0.1 g of polyethylene glycol leveling agent, 0.5 g of p-methoxybenzaldehyde brightener, 2 g of sodium alkyl sulfonate wetting agent, 0.3 g of ascorbic acid antioxidant, 50 g of zinc sulfate, 30 g of sodium chloride, 30 g of boric acid, and 885.1 g of water to mix and prepare a plating solution; adjust the pH value of the plating solution to 5.0, and conduct the plating at 25 ° C and a current density of 2 A / dm 2 Electroplating is carried out under the condition of high temperature to obtain a bright and uniform zinc plating layer.

[0033] Example 2

[0034] A one-liter plating solution is prepared, which includes 2.5 g of ethylenediaminetetraacetic acid complexing agent, 0.5 g of polyethylene glycol leveling agent, 3.0 g of p-methoxybenzaldehyde brightener, 5 g of sodium alkyl sulfonate wetting agent, 5 g of ascorbic acid antioxidant, 50 g of zinc sulfate, 30 g of sodium chloride, 30 g of boric acid, and 874 g of water to obtain a plating solution; the pH value of the plating solution is adjusted to 5.0, and the plating solution is heated at 25°C and a current density of 2 A / dm 2 Electroplating is carried out under the condition of high temperature to obtain a bright and uniform zinc plating layer.

[0035] Example 3

[0036] A one-liter plating solution is prepared, which includes 2.25 g of ethylenediaminetetraacetic acid complexing agent, 0.25 g of polyethylene glycol leveling agent, 2 g of p-methoxybenzaldehyde brightener, 3 g of sodium alkyl sulfonate wetting agent, 3 g of ascorbic acid antioxidant, 50 g of zinc sulfate, 30 g of sodium chloride, 30 g of boric acid, and 879.5 g of water to obtain a plating solution; the pH value of the plating solution is adjusted to 5.0, and the plating solution is heated at 25°C and a current density of 2 A / dm 2 Electroplating is carried out under the condition of high temperature to obtain a bright and uniform zinc plating layer.

[0037] Example 4

[0038] A one-liter plating solution is prepared, which includes 2.25 g of ethylenediaminetetraacetic acid complexing agent, 0.25 g of polyacrylamide leveling agent, 2 g of p-methoxybenzaldehyde brightener, 3 g of sodium alkyl sulfonate wetting agent, 3 g of ascorbic acid antioxidant, 50 g of zinc sulfate, 30 g of sodium chloride, 30 g of boric acid, and 879.5 g of water to obtain a plating solution; the pH value of the plating solution is adjusted to 5.0, and the plating solution is heated at 25°C and a current density of 2 A / dm 2 Electroplating is carried out under the condition of high temperature to obtain a bright and uniform zinc plating layer.

[0039] Example 5

[0040] A one-liter plating solution is prepared, which includes 2.25 g of ethylenediaminetetraacetic acid complexing agent, 0.25 g of polyacrylamide leveling agent, 2 g of p-methoxybenzaldehyde brightener, 3 g of sodium alkyl sulfonate wetting agent, 3 g of ascorbic acid antioxidant, 60 g of zinc sulfate, 20 g of potassium chloride, 20 g of boric acid, and 889.5 g of water to obtain a plating solution; the pH value of the plating solution is adjusted to 5.0, and the plating solution is heated at 25°C and a current density of 2 A / dm 2 Electroplating is carried out under the condition of high temperature to obtain a bright and uniform zinc plating layer.

[0041] Example 6

[0042] A one-liter plating solution is prepared, which includes 2.25 g of ethylenediaminetetraacetic acid complexing agent, 0.25 g of polyacrylamide leveling agent, 1 g of benzylamine brightener and 1 g of p-methoxybenzaldehyde brightener, 3 g of sodium alkyl sulfonate wetting agent, 3 g of ascorbic acid antioxidant, 60 g of zinc sulfate, 20 g of potassium chloride, 20 g of boric acid, and 889.5 g of water to obtain a plating solution; the pH value of the plating solution is adjusted to 5.0, and the plating solution is heated at 25°C and a current density of 2 A / dm 2 Electroplating is carried out under the condition of high temperature to obtain a bright and uniform zinc plating layer.

[0043] Example 7

[0044] A one-liter plating solution is prepared, which includes 2.25 g of ethylenediaminetetraacetic acid complexing agent, 0.25 g of polyacrylamide leveling agent, 1 g of benzyl acetone and 1 g of p-methoxybenzaldehyde brightener, 3 g of sodium alkyl sulfonate wetting agent, 3 g of ascorbic acid antioxidant, 60 g of zinc sulfate, 20 g of potassium chloride, 20 g of boric acid, and 889.5 g of water to obtain a plating solution; the pH value of the plating solution is adjusted to 5.0, and the plating solution is heated at 25°C and a current density of 2 A / dm 2 Electroplating is carried out under the condition of high temperature to obtain a bright and uniform zinc plating layer.

[0045] Comparative Example 1

[0046] Prepare one liter of plating solution by weighing 2 g of ethylenediaminetetraacetic acid complexing agent, 0.1 g of polyethylene glycol leveling agent, 0.5 g of benzyl acetone brightener, 2 g of sodium alkyl sulfonate wetting agent, 0.3 g of ascorbic acid antioxidant, 50 g of zinc sulfate, 30 g of sodium chloride, 30 g of boric acid, and 885.1 g of water to prepare a plating solution; adjust the pH value of the plating solution to 5.0, and conduct the plating at 25 ° C and a current density of 2 A / dm 2 If electroplating is carried out under this condition, a bright and uniform zinc plating layer cannot be obtained.

[0047] Comparative Example 2

[0048] Prepare one liter of plating solution by weighing 2 g of ethylenediaminetetraacetic acid complexing agent, 0.1 g of polyethylene glycol leveling agent, 0.5 g of benzylamine and 0.5 g of benzyl chloride, 2 g of sodium alkyl sulfonate wetting agent, 0.3 g of ascorbic acid antioxidant, 50 g of zinc sulfate, 30 g of sodium chloride, 30 g of boric acid, and 885.1 g of water to prepare a plating solution; adjust the pH value of the plating solution to 5.0, and conduct the plating at 25 ° C and a current density of 2 A / dm 2 If electroplating is carried out under this condition, a bright and uniform zinc plating layer cannot be obtained.

[0049] Test Example 1

[0050] The electroplating solutions prepared in Examples 1 to 7 and Comparative Examples 1 to 2 were subjected to stability tests. The specific experimental results are shown in Table 1.

[0051] Table 1

[0052]

[0053] As can be seen from Table 1, when preparing a cyanide-free electroplating solution, in the stability experiment, the electroplating solution containing the methoxybenzaldehyde brightener is stored for 9 months without precipitation, and the electroplating solution is uniform and unchanged, so the compatibility between the various components of the electroplating solution is good; while in Comparative Examples 1 and 2, the electroplating solutions prepared by adding conventional brighteners but not adding methoxybenzaldehyde brighteners have different degrees of precipitation after 1 week, and cannot be used normally.

[0054] The cyanide-free zinc plating provided by the present application has a significant effect in improving the brightness and uniformity, stability and compatibility of the coating. The use of p-methoxybenzaldehyde as a brightener avoids the environmental and health hazards of cyanide.

[0055] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A novel cyanide-free zinc plating solution formula, characterized in that: The novel cyanide-free zinc plating solution formula comprises the following components by weight: The brightener is selected from at least one of benzalkyne acetone, benzylamine, acetylene alcohol compounds, benzyl chloride, thiourea and its derivatives, and p-methoxybenzaldehyde.

2. The novel cyanide-free zinc plating solution formulation according to claim 1 is characterized in that: The acetylene alcohol compound is selected from at least one of acetylene methanol, 1-ethynyl cyclohexanol and propargyl alcohol.

3. The novel cyanide-free zinc plating solution formulation according to claim 1 is characterized in that: The complexing agent is selected from at least one of ethylenediaminetetraacetic acid, sodium citrate, triethanolamine and glycine.

4. The novel cyanide-free zinc plating solution formulation according to claim 1 is characterized in that: The leveling agent is selected from at least one of polyethylene glycol, polyacrylamide, and sodium N,N-dimethyldithiocarbamate.

5. The novel cyanide-free zinc plating solution formulation according to claim 1 is characterized in that: The wetting agent is selected from sodium alkyl sulfonate and / or sodium alkylbenzene sulfonate.

6. The novel cyanide-free zinc plating solution formulation according to claim 1 is characterized in that: The antioxidant is selected from ascorbic acid and / or sodium metabisulfite.

7. The novel cyanide-free zinc plating solution formulation according to claim 1 is characterized in that: The auxiliary additive is selected from at least one of aluminum salt, zinc salt, potassium salt, ammonium salt and pH regulator.

8. The novel cyanide-free zinc plating solution formulation according to claim 6 is characterized in that: The aluminum salt is selected from at least one of aluminum chloride, aluminum sulfate, and aluminum nitrate; Preferably, the zinc salt is selected from at least one of zinc chloride, zinc sulfate and zinc nitrate.

9. The novel cyanide-free zinc plating solution formulation according to claim 6 is characterized in that: The potassium salt is selected from at least one of potassium chloride, potassium sulfate and potassium nitrate; Preferably, the ammonium salt is selected from at least one of ammonium chloride, ammonium nitrate and ammonium sulfate.

10. The novel cyanide-free zinc plating solution formulation according to claim 6 is characterized in that: The pH regulator is selected from at least one of boric acid, acetic acid, sodium hydroxide and potassium hydroxide.

Citation Information

Patent Citations

  • Additive of sulfuric acid system bright electroplating solution

    CN112725848A

  • Environment-friendly cyanide-free alkaline galvanizing electroplating solution and preparation method and electroplating process thereof

    CN112725849A

  • Acid zinc plating baths and methods for electrodepositing bright zinc deposits

    US4162947A