Conductive acrylic fiber and preparation method thereof
By using DMSO solvent and salts and pyrrole compounds in the treatment solution to form a conductive layer, the problems of unstable conductivity and high preparation cost of conductive fiber materials are solved, and the efficient preparation of conductive acrylic fibers is achieved, which improves its machinery Performance and durability.
Patent Information
- Application Number
- CN202411267886.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-12-03
AI Technical Summary
The problems of existing conductive fiber materials in unstable conductivity, high production cost and difficult to balance mechanical strength and conductive properties limit their application in a wider field.
Using DMSO as a solvent, conductive acrylic fibers are formed by wet spinning and treatment liquid treatment, and salts such as copper sulfate, silver nitrate, nickel sulfate and polypyrrole compounds are used to form a stable conductive layer, combined with water washing, drafting and heat setting treatment , improve the conductivity and mechanical properties of the fibers.
The stable conductivity and mechanical properties of conductive acrylic fibers are achieved, which reduces production costs and improves the durability and application potential of fibers.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of fiber materials, and in particular to a conductive acrylic fiber and a preparation method thereof. Background Art
[0002] With the rapid development of modern science and technology, conductive fibers have shown broad application prospects in the fields of smart textiles, electromagnetic shielding materials, sensors, and medical equipment due to their unique functionality. The conductive fibers currently on the market mainly include metal fibers, carbon-based fibers, and metal-coated fibers. However, these traditional conductive fibers have some inherent defects, such as poor flexibility of metal fibers, unstable conductivity of carbon-based fibers, and poor environmental adaptability of metal-coated fibers. In addition, the production cost of these materials is relatively high, which limits their application in a wider range of fields.
[0003] Conductive acrylic fiber, as a new type of conductive material, has attracted attention due to its excellent softness, cost-effectiveness and stable conductive properties. Existing methods for preparing conductive acrylic fibers usually involve complex chemical reactions and multi-step post-processing processes, which not only increase production costs but also limit the feasibility of large-scale production. In addition, the conductive acrylic fibers prepared by existing methods often find it difficult to achieve an ideal balance between conductive properties and mechanical strength, and their durability needs to be improved. Therefore, developing a simple, cost-effective method for preparing conductive acrylic fibers that can maintain the excellent conductive and mechanical properties of the fibers is of great practical significance for promoting the further application and development of conductive fiber materials. Summary of the invention
[0004] In view of the problems existing in the existing conductive fiber preparation methods, such as unstable product conductivity and high preparation cost, the present invention aims to provide a conductive acrylic fiber and a preparation method thereof.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows: A method for preparing conductive acrylic fiber comprises the following steps: 1) Preparation of spinning solution The acrylic fiber powder is mixed with dimethyl sulfoxide (DMSO) at a weight ratio of 1:1-1:5 to ensure that it is fully dissolved to form a uniform spinning solution. The dissolution process is carried out at room temperature with continuous stirring to promote dissolution for 4-12 hours.
[0006] 2) Wet spinning The spinning solution is extruded through the spinneret and enters the coagulation bath for coagulation and forming to obtain the primary fiber. The coagulation bath consists of deionized water and the temperature is controlled at 20-30℃ to optimize the fiber forming process; 3) Washing and drawing The spun fibers are washed to remove residual solvent and coagulant, the washing temperature is controlled at 20-60°C, the draft ratio is 1.2-1.5, and the draft speed is 20-30m / min to improve the orientation and mechanical properties of the fibers.
[0007] 4) Treatment of treatment fluid One or more salts and pyrrole compounds are prepared into a treatment solution with a concentration of 0.05-1 mol / L, and the stretched fiber is immersed in the treatment solution. The treatment time is controlled at 1-3 hours and the temperature is maintained at 40-60°C to ensure that a uniform conductive layer is formed on the fiber surface.
[0008] The salts are copper sulfate, silver nitrate, nickel sulfate and the like, and the pyrrole compounds are polypyrrole and the like.
[0009] 5) Post-processing The fibers treated with the treatment liquid are fully washed with water to remove the residual treatment liquid, and then the fibers are subjected to heat setting treatment at a temperature of 120-160° C. for 5-30 minutes to stabilize the fiber structure.
[0010] 6) Drying and winding The fiber is dried in a hot air circulation drying oven at a drying temperature of 60-80°C until the moisture content of the fiber is less than 5%.
[0011] The dried fiber is wound by a winder at a speed of 20-30 m / min to form a fiber roll suitable for subsequent processing and application.
[0012] The present invention has the following beneficial effects: 1. Using DMSO as a solvent can effectively dissolve acrylic fiber powder to form a uniform spinning solution.
[0013] 2. The treatment solution of the present invention is composed of one or more salts such as copper sulfate, silver nitrate, nickel sulfate and pyrrole compounds. After the fiber is treated with the treatment solution, a stable conductive layer can be formed to improve the conductive performance of the fiber. DETAILED DESCRIPTION
[0014] The present invention is described in more detail below through specific examples, but the present invention is not limited thereto. Example
[0015] A method for preparing conductive acrylic fiber comprises the following steps: 1) Preparation of spinning solution The acrylic fiber powder was mixed with DMSO in a weight ratio of 1:4 to ensure that it was fully dissolved to form a uniform spinning solution. The dissolution process was carried out at room temperature with continuous stirring to promote dissolution for 6 hours.
[0016] 2) Wet spinning The prepared spinning solution is extruded through the spinneret and enters the coagulation bath for coagulation and forming to obtain the nascent fiber. The coagulation bath consists of deionized water and the temperature is controlled at 20°C to optimize the fiber forming process.
[0017] 3) Washing and drawing The nascent fiber was washed to remove residual solvent and coagulant, and the washing temperature was controlled at 20° C. The draft ratio was 1.2 and the draft speed was 20 m / min to improve the orientation and mechanical properties of the fiber.
[0018] 4) Treatment of treatment fluid: The drawn fiber is immersed in a treatment solution of copper sulfate, silver nitrate and polypyrrole, wherein the mass ratio of copper sulfate, silver nitrate and polypyrrole is 1:3:1 and the concentration of the treatment solution is 0.1 mol / L. The treatment time is controlled at 1 hour and the temperature is maintained at 60°C to ensure that a uniform conductive layer is formed on the fiber surface.
[0019] 5) Post-processing The treated fibers were fully washed to remove the residual treatment solution, and then heat-set at 140°C for 5 minutes to stabilize the fiber structure.
[0020] 6) Drying and winding The fiber was placed in a hot air circulation drying oven for drying at a temperature of 60°C until the moisture content of the fiber was less than 5%.
[0021] The dried fiber is wound by a winder at a speed of 20 m / min to form a fiber roll suitable for subsequent processing and application. Example
[0022] A method for preparing conductive acrylic fiber comprises the following steps: 1) Preparation of spinning solution The acrylic fiber powder was mixed with DMSO in a weight ratio of 1:3 to ensure that it was fully dissolved to form a uniform spinning solution. The dissolution process was carried out at room temperature with continuous stirring to promote dissolution for 8 hours.
[0023] 2) Wet spinning The prepared spinning solution is extruded through the spinneret and enters the coagulation bath for coagulation and forming to obtain the nascent fiber. The coagulation bath consists of deionized water and the temperature is controlled at 20°C to optimize the fiber forming process.
[0024] 3) Washing and drawing: The spun fibers were washed to remove residual solvent and coagulant, and the washing temperature was controlled at 20° C. The draft ratio was 1.2 and the draft speed was 20 m / min to improve the orientation and mechanical properties of the fibers.
[0025] 4) Treatment of treatment fluid The drawn fiber is immersed in a treatment solution prepared with copper sulfate and nickel sulfate, wherein the mass ratio of copper sulfate to nickel sulfate is 1:3 and the concentration of the treatment solution is 0.5 M. The treatment time is controlled at 2 hours and the temperature is maintained at 60°C to ensure that a uniform conductive layer is formed on the fiber surface.
[0026] 5) Post-processing The treated fibers were fully washed to remove the residual treatment solution, and then heat-set at 140°C for 5 minutes to stabilize the fiber structure.
[0027] 6) Drying and winding The fiber was placed in a hot air circulation drying oven for drying at a temperature of 60°C until the moisture content of the fiber was less than 5%.
[0028] The dried fiber is wound by a winder at a speed of 20 m / min to form a fiber roll suitable for subsequent processing and application. Example
[0029] A method for preparing conductive acrylic fiber comprises the following steps: 1) Preparation of spinning solution The acrylic fiber powder was mixed with DMSO in a weight ratio of 1:5 to ensure that it was fully dissolved to form a uniform spinning solution. The dissolution process was carried out at room temperature with continuous stirring to promote dissolution for 10 hours.
[0030] 2) Wet spinning The prepared spinning solution is extruded through the spinneret and enters the coagulation bath for coagulation and forming to obtain the nascent fiber. The coagulation bath consists of deionized water and the temperature is controlled at 25°C to optimize the fiber forming process.
[0031] 3) Washing and drawing The nascent fiber was washed to remove residual solvent and coagulant, and the washing temperature was controlled at 30°C. The draft ratio was 15 and the draft speed was 30m / min to improve the orientation and mechanical properties of the fiber.
[0032] 4) Treatment of treatment fluid: The drawn fiber was immersed in a treatment solution of copper sulfate, nickel sulfate and polypyrrole, where the mass ratio of copper sulfate, silver nitrate and polypyrrole was 1:3:1 and the concentration of the treatment solution was 0.8 mol / L. The treatment time was controlled at 3 hours and the temperature was maintained at 50°C to ensure that a uniform conductive layer was formed on the fiber surface.
[0033] 5) Post-processing The treated fibers were fully washed to remove the residual treatment solution, and then the fibers were heat-set at 120°C for 25 minutes to stabilize the fiber structure.
[0034] 6) Drying and winding The fiber was placed in a hot air circulation drying oven for drying at a temperature of 70°C until the moisture content of the fiber was less than 5%.
[0035] The dried fiber is wound by a winder at a speed of 30m / min to form a fiber roll suitable for subsequent processing and application.
Claims
1. A method for preparing conductive acrylic fiber, It is characterized in that The following steps are involved: 1) Preparation of spinning solution Mixing and dissolving acrylic fiber powder and dimethyl sulfoxide in a weight ratio of 1:1-1:5 to form a uniform spinning solution; 2) Wet spinning The spinning solution is extruded through a spinneret hole and enters a coagulation bath composed of deionized water for coagulation and forming to obtain primary fibers; 3) Washing and drawing The spun fiber is washed to remove residual solvent and coagulant, the washing temperature is controlled at 20-60°C, the draft ratio is 1.2-1.5, and the draft speed is 20-30m / min; 4) Treatment of treatment fluid One or more of the salts and pyrrole compounds are prepared into a treatment solution with a concentration of 0.05-1 mol / L, and the drawn fiber is immersed in the treatment solution. The treatment time is controlled to be 1-3 hours, and the temperature is maintained at 40-60°C; 5) Post-processing The fibers treated with the treatment liquid are fully washed with water to remove the residual treatment liquid, and then the fibers are heat-set at a temperature of 120-160°C for 5-30 minutes; 6) Drying and winding The fiber is placed in a hot air circulation drying oven for drying at a drying temperature of 60-80°C, and the dried fiber is wound by a winder.
2. A method for preparing a conductive acrylic fiber according to claim 1, It is characterized in that The dissolution in step 1) is carried out under stirring at room temperature for 4-12 hours.
3. A method for preparing a conductive acrylic fiber according to claim 1, It is characterized in that Step 2) The temperature of the coagulation bath is 20-30°C.
4. A method for preparing a conductive acrylic fiber according to claim 1, It is characterized in that The salt in step 4) is copper sulfate, silver nitrate or nickel sulfate, and the pyrrole compound is polypyrrole.
5. A method for preparing a conductive acrylic fiber according to claim 1, It is characterized in that Step 6) Drying until the moisture content of the fiber is less than 5%.
6. A method for preparing a conductive acrylic fiber according to claim 1, It is characterized in that The winding speed in step 6) is 20-30 m / min.