Tencel viscose flax slubbed fabric
By adjusting the proportion and weaving process of viscose fiber, tensile fiber and flax fiber, the shrinkage rate fluctuation and strong decrease of viscose linen-blend bamboo joint fabrics are solved, and the stability and quality of the fabric are improved, meeting high quality Textile demand.
Patent Information
- Application Number
- CN202411270418.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-12-03
AI Technical Summary
The existing viscose linen blended bamboo fabrics have large fluctuations in shrinkage and strong decreases due to high content of viscose fiber, especially in humid environments, which affects clothing size control and deep processing, resulting in waste and loss.
Tencel viscose linen bamboo node cloth is used to mix spinning through an air-flow spinning machine to adjust the proportion of viscose, tencel fiber and flax fiber, and weave it plain weaving, and density control and pre-shrinkage to stabilize the shrinkage of the fabric. rate and form.
It effectively reduces the fluctuation of the shrinkage rate of the fabric, enhances the strength and durability of the fabric, improves the quality and feel, and meets the needs of high-quality fabrics.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of textiles, in particular to tencel viscose linen slub fabric. Background Art
[0002] The viscose and linen blended slub yarn fabrics on the current market are popular among customers for their unique style and quality. However, the characteristics of viscose fiber bring about significant shrinkage and strength reduction problems, especially in humid environments, which are more serious, making it difficult to control the size of clothing, affecting further processing and causing waste and loss. Summary of the invention
[0003] 1. Technical issues to be resolved
[0004] In view of the deficiencies of the prior art, the present invention provides a Tencel viscose linen slub fabric.
[0005] (II) Technical solution
[0006] To achieve the above object, the present invention provides the following technical solution: Tencel viscose linen slub fabric, comprising the following raw materials in the following weight proportions:
[0007] Viscose 40-50%;
[0008] Tencel fiber 30-40%;
[0009] Flax fiber 20%;
[0010] The air spinning machine is used for mixed spinning, so that the viscose fiber, tencel fiber and flax fiber are fully mixed and formed into slub yarn.
[0011] Preferably, the Tencel viscose linen slub fabric comprises the following raw materials in proportion by weight:
[0012] Viscose 40%;
[0013] Tencel fiber 40%;
[0014] Flax fiber 20%;
[0015] The slub yarn is woven by a plain weave method, with the warp density controlled at 130 strands / 10 cm and the weft density controlled at 126 strands / 10 cm to form a grey cloth.
[0016] Preferably, the viscose fiber is 83tex.
[0017] Preferably, the Tencel fiber is 38tex.
[0018] (III) Beneficial effects
[0019] Compared with the prior art, the present invention provides a Tencel viscose linen slub fabric, which has the following beneficial effects:
[0020] Improved shrinkage stability: By adjusting the ratio of viscose fiber and Tencel fiber, the shrinkage fluctuation of the fabric is effectively reduced.
[0021] Enhance fabric strength and durability: The introduction of Tencel fiber greatly enhances the strength of the fabric, especially the fiber strength in a wet state is significantly better than that of fabrics with a high content of viscose fiber.
[0022] Improve fabric quality: Due to the characteristics of Tencel fiber, the drape and feel of the fabric are significantly improved, making the fabric more high-end and meeting customers' demand for high-quality fabrics. DETAILED DESCRIPTION
[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0024] The previous sample specifications were: 83tex viscose-linen blended slub yarn, composed of 80% viscose fiber, 20% linen fiber, warp density of 130 strands / 10cm, weft density of 126 strands / 10cm plain weave. However, due to the high content of viscose fiber, the shrinkage rate fluctuated (-7% to -13%), the strength decreased, and other problems affected the further processing.
[0025] The tencel viscose linen slub fabric comprises the following raw materials in proportion by weight:
[0026] Viscose 40-50%;
[0027] Tencel fiber 30-40%;
[0028] Flax fiber 20%;
[0029] The air spinning machine is used for mixed spinning, so that the viscose fiber, tencel fiber and flax fiber are fully mixed and formed into slub yarn.
[0030] Embodiment 1:
[0031] Adjust the ratio to 40% viscose fiber, 40% tencel fiber, and 20% flax fiber;
[0032] The slub yarn is woven by plain weaving, the warp density is controlled at 130 strands / 10cm, and the weft density is controlled at 126 strands / 10cm to form a grey cloth. The grey cloth is pre-shrunk to achieve the best shrinkage state, and then subjected to shaping treatment to ensure the dimensional stability and shape of the fabric. The shrinkage rate of the fabric is stabilized between -5% and -7%, showing a relatively ideal stability.
[0033] Embodiment 2:
[0034] 50% viscose fiber, 30% tencel fiber, and 20% flax fiber were selected;
[0035] The bamboo yarn is woven using a plain weave method, with the warp density controlled at 130 strands / 10cm and the weft density controlled at 126 strands / 10cm to form a grey cloth. The grey cloth is pre-shrunk to achieve the best shrinkage state, and then subjected to a shaping treatment to ensure the dimensional stability and shape of the fabric. The shrinkage rate of the fabric is controlled between -6% and -10%, which is an improvement compared to the initial stage, but still not the best effect.
[0036] In the above embodiment, the viscose fiber is 83tex, and the tencel fiber is 38tex.
[0037] This technical solution solves the post-processing problem of bamboo fabrics due to high shrinkage and reduced strength by accurately adjusting the ratio of viscose fiber and tencel fiber, and meets the market demand for high-quality and stable textiles. The above improvements have achieved remarkable results.
[0038] In order to explain in detail the possible application scenarios, technical principles, specific schemes that can be implemented, and the purposes and effects that can be achieved, the following is a detailed description in conjunction with the specific embodiments listed. The embodiments described herein are only used to more clearly illustrate the technical solutions of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.
[0039] Reference to "embodiment" herein means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The term "embodiment" appearing in various places in the specification does not necessarily refer to the same embodiment, nor does it particularly limit its independence or association with other embodiments. In principle, in the present application, as long as there is no technical contradiction or conflict, the various technical features mentioned in the embodiments can be combined in any way to form a corresponding implementable technical solution.
[0040] Unless otherwise defined, the technical terms used in this document have the same meanings as those generally understood by those skilled in the art to which this application belongs; the use of relevant terms in this document is only for describing specific embodiments and is not intended to limit this application.
[0041] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. Tencel viscose linen slub fabric, characterized in that: The raw materials include the following weight proportions: Viscose 40-50%; Tencel fiber 30-40%; Flax fiber 20%; The air spinning machine is used for mixed spinning, so that the viscose fiber, tencel fiber and flax fiber are fully mixed and formed into slub yarn.
2. The Tencel viscose linen slub fabric according to claim 1, characterized in that: The raw materials include the following weight proportions: Viscose 40%; Tencel fiber 40%; Flax fiber 20%; The slub yarn is woven by a plain weave method, with the warp density controlled at 130 strands / 10 cm and the weft density controlled at 126 strands / 10 cm to form a grey cloth.
3. The Tencel viscose linen slub fabric according to claim 2, characterized in that: The viscose fiber is 83tex.
4. The Tencel viscose linen slub fabric according to claim 3, characterized in that: The tencel fiber is 38tex.
Citation Information
Patent Citations
Flax scribbled yarn and its production
CN101074508A
Method for producing multicolor composite slub or satin color yarn series, shell fabric and yarn
CN102677247A
Cotton, viscose and linen rotor spinning fabric manufacturing method
CN103849980A
Degummed and bleached linen and viscose siro spinning bunchy blended yarn and production process thereof
CN106120054A
Rotor spinning slub yarn and production method thereof
CN115652494A