Preparation method of simple, green and degradable bamboo leather material and product

By combining bamboo fibers with polyurethane and polylactic acid, biodegradable bamboo cellulose composite materials are prepared through blending and hot pressing processes, solving the problems of environmental pollution and poor degradability of synthetic leather materials, and providing an environmentally friendly and low-quality Cost of leather alternatives.

CN119061585APending Publication Date: 2024-12-03BEIJING INST OF CLOTHING TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411254493.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing synthetic leather materials use a large amount of chemicals during the production process and have poor degradability, resulting in environmental pollution problems and lack of environmentally friendly alternatives.

Method used

Using bamboo fibers as raw materials, combined with polyurethane and polylactic acid through blending and hot pressing processes, a biodegradable bamboo cellulose composite material is prepared as a replacement for leather.

Benefits of technology

It realizes environmentally friendly and low-cost leather alternatives, reduces environmental pollution, has good flexibility, hydrophobic properties, and has excellent biodegradable properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061585A_ABST
    Figure CN119061585A_ABST
Patent Text Reader

Abstract

The invention discloses a simple, green and degradable bamboo leather material preparation method and a product, and the method comprises the following steps: preparing a bamboo fiber aggregate from dried bamboo through a physical or green chemical method, drying the bamboo fiber aggregate to a constant weight for later use, putting the bamboo fiber aggregate into a beaker, adding deionized water to dissociate bamboo fibers in the beaker, and carrying out ultrasonic treatment on the bamboo fiber aggregate to obtain the bamboo leather material. Filtering after dissociation is completed, taking the dissociated bamboo fibers, standing for later use, sequentially adding polyurethane and polylactic acid into a solvent, heating, stirring and dissolving to obtain a glue binding matrix liquid, uniformly mixing the dissociated bamboo fibers with the prepared glue binding matrix liquid through a stirrer, and carrying out drying, so as to obtain a glue binding material; the preparation method comprises the following steps: preparing a composite bamboo fiber material containing polyurethane and polylactic acid, pouring the composite bamboo fiber material containing polyurethane and polylactic acid into a mold to obtain a to-be-hot-pressed composite bamboo fiber material containing polyurethane and polylactic acid, carrying out hot pressing, and carrying out hot pressing on the to-be-hot-pressed composite bamboo fiber material to obtain the biodegradable bamboo cellulose leather material. And the environmental pollution is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of light industry textiles, and in particular to a preparation method and product of a simple, green and degradable bamboo leather material. Background Art

[0002] With the introduction of animal protection laws and people's increasing awareness of animal protection, animal leather has gradually become history. The manufacture of synthetic leather does not require the use of animal leather, avoiding animal harm and environmental pollution during leather processing. Synthetic leather has a lower cost, and synthetic leather products such as shoes and handbags have a lower cost. The emergence of synthetic leather meets people's growing demand for leather and has gradually developed into a trend.

[0003] At present, synthetic leather materials require the use of more chemical substances in the production process, so they are not environmentally friendly compared to natural materials, and their degradability is poor. my country is rich in bamboo resources, bamboo has a short growth cycle, and bamboo is a renewable resource with good degradability. In this case, bamboo fiber is used as the raw material, and after a simple blending and hot pressing process, it is compounded with a glue-bonded matrix liquid to prepare a leather-like bamboo cellulose composite material, which is a good potential substitute for leather. In addition, bamboo cellulose molecules have a large number of modifiable groups. After being modified by hydrophobicity, dyeing, antibacterial and conductivity, the product can not only meet the basic performance requirements of synthetic leather, but also has good flexibility, hydrophobicity and excellent biodegradability. It has huge potential application prospects in textiles, clothing, etc. Summary of the invention

[0004] The purpose of this section is to summarize some aspects of the embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.

[0005] Therefore, the purpose of the present invention is to provide a simple, green and degradable bamboo leather material preparation method and product, realize the replacement of synthetic leather, and develop new uses of bamboo fiber, reducing environmental pollution.

[0006] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:

[0007] A method for preparing a simple, green and degradable bamboo leather material, comprising:

[0008] S1. Preparation of bamboo fiber: preparing bamboo fiber aggregates from dried bamboo by physical or green chemical methods, drying to constant weight for later use, wherein the bamboo fiber aggregates are in block shape;

[0009] S2, bamboo fiber dissociation: put the bamboo fiber aggregate into a beaker, add deionized water to dissociate the bamboo fiber in the beaker, and in order to obtain a more homogeneous bamboo fiber solution, add deionized water in batches and stir, and the final volume of deionized water is 10-15 times the volume of bamboo fiber. After the dissociation is completed, filter and take the dissociated bamboo fiber and set aside;

[0010] S3, preparing a glue-binding matrix liquid: adding polyurethane and polylactic acid to a solvent in sequence, heating and stirring to dissolve, to obtain a glue-binding matrix liquid, wherein the dissolution temperature of polyurethane is 35-40° C., and the dissolution temperature of polylactic acid is 45-60° C.;

[0011] S4, blending: the bamboo fiber dissociated in step S2 and the adhesive-bonded matrix liquid prepared in step S3 are uniformly mixed by a stirrer, and after completion, poured into a mold to obtain a composite bamboo fiber material to be hot-pressed containing polyurethane and polylactic acid, and then hot-pressed;

[0012] S5, hot pressing preparation: hot pressing the composite bamboo fiber material to be hot pressed in step S4 at 10 min / mm to obtain a biodegradable bamboo fiber leather material.

[0013] As a preferred embodiment of the method for preparing a simple, green and degradable bamboo leather material described in the present invention, in step S1, the specific steps of preparing bamboo fiber from dried bamboo by a chemical method are as follows: the bamboo is split into two halves or pierced from the center, soaked in water, broomed three times, and then softened, fiberized, and steamed in a cooking liquid, neutralized and washed with a sulfuric acid solution or a hydrochloric acid solution, and then washed, degummed, dehydrated, and dried to obtain bamboo raw fibers.

[0014] As a preferred embodiment of the method for preparing a simple, green and degradable bamboo leather material according to the present invention, in step S2, the time for deionized water to dissociate the bamboo fibers is 3-6 hours.

[0015] As a preferred embodiment of the method for preparing a simple, green and degradable bamboo leather material described in the present invention, in step S3, the adhesive bonding matrix liquid includes type A bonding matrix and type B bonding matrix, and the weight ratio of type A bonding matrix to type B bonding matrix is ​​1:3.

[0016] As a preferred solution of the method for preparing a simple, green and degradable bamboo leather material described in the present invention, the solid content of the adhesive bonding matrix liquid in the adhesive bonding matrix liquid is 1-5%.

[0017] As a preferred embodiment of the method for preparing a simple, green and degradable bamboo leather material described in the present invention, in step S3, the heating conditions are: heating for 10 min to 20 min at an initial temperature of 30°C to 60°C and a stirring speed of 0 to 1600 r / min.

[0018] As a preferred embodiment of the method for preparing a simple, green and degradable bamboo leather material described in the present invention, in step S5, the hot pressing conditions are: hot pressing for 8 minutes to 20 minutes at a temperature of 80°C to 150°C and a pressure of 5KPa to 20KPa.

[0019] As a preferred embodiment of the method for preparing a simple, green and degradable bamboo leather material according to the present invention, in step S3, the bamboo fiber is one or more of moso bamboo, cycad bamboo, tea stem bamboo and green bamboo.

[0020] As a preferred solution of the method for preparing a simple, green and degradable bamboo leather material described in the present invention, the weight percentage of bamboo fiber content in the prepared leather-like bamboo cellulose composite material is 20%-65%.

[0021] As a preferred embodiment of the method for preparing a simple, green and degradable bamboo leather material according to the present invention, in step S1, bamboo fiber is prepared from moso bamboo and / or green bamboo by a chemical method.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The present invention uses bamboo as raw material, which is abundant and renewable. The production cost is low, and a new use of bamboo is developed. In the production process, no excessive chemical reagents are used, the production process is simple, the cost is low, and environmental pollution is reduced. In addition, the leather-like bamboo cellulose composite material prepared by using bamboo fiber as raw material, polyurethane and polylactic acid as auxiliary materials is environmentally friendly and green material. Bamboo fiber and polylactic acid have good degradability. Compared with synthetic leather, it is green and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the present invention will be described in detail below in combination with the accompanying drawings and detailed embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:

[0025] Figure 1 This is a flow chart of a method for preparing a simple, green and degradable bamboo leather material according to the present invention;

[0026] Figure 2 Schematic diagram of sample sheets P1, P2 and P3 provided by the present invention before and after degradation;

[0027] Figure 3 This is a front SEM photo of the sample sheet P1 provided by the present invention after being degraded;

[0028] Figure 4 This is a SEM photograph of the reverse side of the degradable sample sheet P1 provided by the present invention. DETAILED DESCRIPTION

[0029] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0030] Secondly, the present invention is described in detail with reference to schematic diagrams. When describing the embodiments of the present invention in detail, for the sake of convenience, the cross-sectional diagrams showing the device structure will not be partially enlarged according to the general scale, and the schematic diagrams are only examples, which should not limit the scope of protection of the present invention. In addition, in actual production, the three-dimensional dimensions of length, width and depth should be included.

[0031] In order to make the objectives, technical solutions and advantages of the present invention more clear, the embodiments of the present invention will be further described in detail below with reference to the accompanying drawings.

[0032] The present invention provides a simple, green and degradable bamboo leather material preparation method and product, which realizes the replacement of synthetic leather, develops new uses of bamboo fiber, and reduces environmental pollution. The process routes of the simple, green and degradable bamboo leather material preparation method in the following embodiments are as follows: Figure 1 shown.

[0033] Example 1

[0034] like Figure 1 As shown, a simple, green and degradable method for preparing bamboo leather material comprises:

[0035] S1. Preparation of bamboo fiber: preparing bamboo fiber aggregates from dried bamboo by physical or green chemical methods, drying to constant weight for later use, wherein the bamboo fiber aggregates are in block shape;

[0036] S2, bamboo fiber dissociation: take bamboo fiber aggregates and put them into a beaker, add deionized water to dissociate the bamboo fiber aggregates in the beaker, the time for dissociating the bamboo fiber is 3.5 hours, filter after the dissociation, take the dissociated bamboo fiber, and set aside;

[0037] S3, preparing adhesive bonding matrix liquid: adding polyurethane and polylactic acid to a solvent in sequence, and heating and stirring to dissolve for 10 minutes at an initial temperature of 30°C and a stirring speed of 800 r / min to obtain an adhesive bonding matrix liquid, wherein the dissolution temperature of polyurethane is 35-40°C, and the dissolution temperature of polylactic acid is 45-60°C;

[0038] S4, blending: the bamboo fiber dissociated in step S2 and the adhesive-bonded matrix liquid prepared in step S3 are uniformly mixed by a stirrer, and after completion, poured into a mold to obtain a composite bamboo fiber material to be hot-pressed containing polyurethane and polylactic acid, and then hot-pressed;

[0039] S5, hot pressing preparation: hot pressing the composite bamboo fiber material to be hot pressed in step S4 at a speed of 10 mm / min at a temperature of 80° C. and a pressure of 5 KPa for 8 minutes to obtain a biodegradable bamboo fiber leather material.

[0040] Example 2

[0041] A method for preparing a simple, green and degradable bamboo leather material, comprising:

[0042] S1. Preparation of bamboo fiber: preparing bamboo fiber aggregates from dried bamboo by physical or green chemical methods, drying to constant weight for later use, wherein the bamboo fiber aggregates are in block shape;

[0043] S2, bamboo fiber dissociation: take bamboo fiber aggregates and put them into a beaker, add deionized water to dissociate the bamboo fiber aggregates in the beaker, the time for dissociating the bamboo fiber is 4 hours, filter after the dissociation, take the dissociated bamboo fiber, and set aside;

[0044] S3, preparing adhesive bonding matrix liquid: adding polyurethane and polylactic acid to the solvent in sequence, and heating and stirring to dissolve for 13 minutes at an initial temperature of 40° C. and a stirring speed of 800 r / min to obtain an adhesive bonding matrix liquid;

[0045] S4, blending: the bamboo fiber dissociated in step S2 and the adhesive-bonded matrix liquid prepared in step S3 are uniformly mixed by a stirrer, and after completion, poured into a mold to obtain a composite bamboo fiber material to be hot-pressed containing polyurethane and polylactic acid, and then hot-pressed;

[0046] S5, hot pressing preparation: hot pressing the composite bamboo fiber material to be hot pressed in step S4 at a speed of 10 mm / min at a temperature of 95° C. and a pressure of 8 KPa for 10 min to obtain a biodegradable bamboo fiber leather material.

[0047] Example 3

[0048] A method for preparing a simple, green and degradable bamboo leather material, comprising:

[0049] S1. Preparation of bamboo fiber: preparing bamboo fiber aggregates from dried bamboo by physical or green chemical methods, drying to constant weight for later use, wherein the bamboo fiber aggregates are in block shape;

[0050] S2, bamboo fiber dissociation: put bamboo fiber aggregates into a beaker, add deionized water to dissociate the bamboo fiber aggregates in the beaker, the time for dissociating the bamboo fiber aggregates is 4.5 hours, filter after the dissociation is completed, take the dissociated bamboo fibers, and set aside;

[0051] S3, preparing adhesive bonding matrix liquid: adding polyurethane and polylactic acid to the solvent in sequence, and heating and stirring to dissolve for 15 minutes at an initial temperature of 45° C. and a stirring speed of 800 r / min to obtain an adhesive bonding matrix liquid;

[0052] S4, blending: the bamboo fiber dissociated in step S2 and the adhesive-bonded matrix liquid prepared in step S3 are uniformly mixed by a stirrer, and after completion, poured into a mold to obtain a composite bamboo fiber material to be hot-pressed containing polyurethane and polylactic acid, and then hot-pressed;

[0053] S5, hot pressing preparation: hot pressing the composite bamboo fiber material to be hot pressed in step S4 at a speed of 10 mm / min at a temperature of 100° C. and a pressure of 10 KPa for 13 minutes to obtain a biodegradable bamboo fiber leather material.

[0054] Example 4

[0055] A method for preparing a simple, green and degradable bamboo leather material, comprising:

[0056] S1. Preparation of bamboo fiber: preparing bamboo fiber aggregates from dried bamboo by physical or green chemical methods, drying to constant weight for later use, wherein the bamboo fiber aggregates are in block shape;

[0057] S2, bamboo fiber dissociation: take bamboo fiber aggregates and put them into a beaker, add deionized water to dissociate the bamboo fiber aggregates in the beaker, the time for dissociating the bamboo fiber is 5 hours, filter after the dissociation, take the dissociated bamboo fiber, and set aside;

[0058] S3, preparing adhesive bonding matrix liquid: adding polyurethane and polylactic acid to the solvent in sequence, and heating and stirring to dissolve for 20 minutes at an initial temperature of 50° C. and a stirring speed of 1000 r / min to obtain an adhesive bonding matrix liquid;

[0059] S4, blending: the bamboo fiber dissociated in step S2 and the adhesive-bonded matrix liquid prepared in step S3 are uniformly mixed by a stirrer, and after completion, poured into a mold to obtain a composite bamboo fiber material to be hot-pressed containing polyurethane and polylactic acid, and then hot-pressed;

[0060] S5, hot pressing preparation: hot pressing the composite bamboo fiber material to be hot pressed in step S4 at a speed of 10 mm / min at a temperature of 110° C. and a pressure of 13 KPa for 15 minutes to obtain a biodegradable bamboo fiber leather material.

[0061] Example 5

[0062] A method for preparing a simple, green and degradable bamboo leather material, comprising:

[0063] S1. Preparation of bamboo fiber: preparing bamboo fiber aggregates from dried bamboo by physical or green chemical methods, drying to constant weight for later use, wherein the bamboo fiber aggregates are in block shape;

[0064] S2, bamboo fiber dissociation: take bamboo fiber aggregates and put them into a beaker, add deionized water to dissociate the bamboo fiber aggregates in the beaker, the time for dissociating the bamboo fiber is 6 hours, filter after the dissociation, take the dissociated bamboo fiber, and set aside;

[0065] S3, preparing adhesive bonding matrix liquid: adding polyurethane and polylactic acid to the solvent in sequence, and heating and stirring to dissolve for 25 minutes at an initial temperature of 60° C. and a stirring speed of 1200 r / min to obtain an adhesive bonding matrix liquid;

[0066] S4, blending: the bamboo fiber dissociated in step S2 and the adhesive-bonded matrix liquid prepared in step S3 are uniformly mixed by a stirrer, and after completion, poured into a mold to obtain a composite bamboo fiber material to be hot-pressed containing polyurethane and polylactic acid, and then hot-pressed;

[0067] S5, hot pressing preparation: hot pressing the composite bamboo fiber material to be hot pressed in step S4 at a speed of 10 mm / min at a temperature of 120° C. and a pressure of 15 KPa for 20 minutes to obtain a biodegradable bamboo fiber leather material.

[0068] The invention uses bamboo as raw material, which is abundant and renewable. The production cost is low, and a new use of bamboo is developed. In the production process, no excessive chemical reagents are used, the production process is simple, the cost is low, and environmental pollution is reduced. The leather-like bamboo cellulose composite material is prepared by using bamboo fiber as raw material and polyurethane and polylactic acid as adhesives. Both are environmentally friendly green materials. Bamboo fiber and polylactic acid have good degradability. Compared with synthetic leather, it is green and environmentally friendly.

[0069] In order to verify the degradability of the bamboo leather material prepared by the present invention, the following method was used for verification:

[0070] The three sample pieces P1 (by mass ratio: 53% bamboo fiber aggregate, 35% polyurethane, 12% polylactic acid), P2 (by mass ratio: 32% bamboo fiber aggregate, 50% polyurethane, 18% polylactic acid) and P3 (by mass ratio: 18% bamboo fiber aggregate, 62% polyurethane, 30% polylactic acid) prepared in Example 1 of the present invention were cut, dried to constant weight (W0), and buried in 250g compost soil with a pH value of 6.5-7.0 and a humidity of 25%. The experiment was carried out in a simulated natural environment with a temperature of 18°C ​​and an ambient humidity of 25%. After three months, the degradation experiment was terminated, the samples were taken out of the soil, repeatedly washed with deionized water, and finally placed in an oven at 40°C to air dry to constant weight (W). After 90 days, the degradation percentage of the material was calculated as follows:

[0071]

[0072] In the formula, W0 is the initial dry weight of the leather sheet, and W is the dry weight of the leather sheet.

[0073] The pictures of samples P1, P2 and P3 before and after degradation are as follows Figure 2 As shown, after calculation, the biodegradation rate of sample P1 is 23.41%, the biodegradation rate of sample P2 is 16.74%, and the biodegradation rate of sample P3 is 7.30%. The biodegradation performance of P1 (23.41%) is the best. The main reason is that when bamboo fiber aggregate / polyurethane / polylactic acid is prepared into a composite material, many micropores will be formed inside the composite material. Water and microorganisms can enter the interior of the composite material through the micropores, and the polylactic acid in the composite material is constantly hydrolyzed and degraded. On the other hand, the change in moisture in the soil causes the swelling and shrinkage of bamboo fibers, which leads to the destruction of the bonding interface between polyurethane / polylactic acid and bamboo fiber aggregates. Moisture and microorganisms can easily enter the interior of the composite material through the destroyed interface, causing the polylactic acid to hydrolyze and degrade. The loss of soluble products formed by the hydrolysis and degradation of polylactic acid leads to a reduction in the quality of the composite material (such as Figure 3 and Figure 4 ). At the same time, the hemicellulose and cellulose of the bamboo fiber aggregates in the bamboo fiber aggregate / polyurethane / polylactic acid composite material are easily decomposed by brown rot fungi, while the lignin is easily decomposed by white rot fungi. Therefore, when the bamboo fiber aggregate / polylactic acid biodegradable composite material is buried in the soil, under certain temperature and humidity, the bamboo fiber aggregates are easily decomposed by brown rot fungi and white rot fungi, which will also lead to an increase in the mass loss rate of the bamboo fiber aggregate / polyurethane / polylactic acid composite material and an improvement in degradation performance.

[0074] Although the present invention has been described above with reference to the embodiments, various modifications may be made thereto and parts thereof may be replaced by equivalents without departing from the scope of the present invention. In particular, as long as there is no structural conflict, the various features in the embodiments disclosed in the present invention may be used in combination with each other in any manner, and the fact that these combinations are not exhaustively described in this specification is only for the sake of omitting space and saving resources. Therefore, the present invention is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

Claims

1. A method for preparing a simple, green and degradable bamboo leather material, characterized in that: include: S1. Preparation of bamboo fiber: preparing bamboo fiber aggregates from dried bamboo by physical or green chemical methods, drying to constant weight for later use, wherein the bamboo fiber aggregates are in block shape; S2, bamboo fiber dissociation: put bamboo fiber aggregates into a beaker, add deionized water to dissociate the bamboo fiber aggregates in the beaker, and in order to obtain a more homogeneous bamboo fiber solution, add deionized water in batches and stir, and the final volume of deionized water is 10-15 times the volume of bamboo fiber. After the dissociation is completed, filter, take the dissociated bamboo fiber, and set aside; S3, preparing a glue-binding matrix liquid: adding polyurethane and polylactic acid to a solvent in sequence, heating and stirring to dissolve, to obtain a glue-binding matrix liquid, wherein the dissolution temperature of polyurethane is 35-40° C., and the dissolution temperature of polylactic acid is 45-60° C.; S4, blending: the bamboo fiber dissociated in step S2 and the adhesive-bonded matrix liquid prepared in step S3 are uniformly mixed by a stirrer, and after completion, poured into a mold to obtain a composite bamboo fiber material to be hot-pressed containing polyurethane and polylactic acid, and then hot-pressed; S5, hot pressing preparation: The composite bamboo fiber material to be hot pressed in step S4 is hot pressed at 10 min / mm to obtain a biodegradable bamboo fiber leather material.

2. The method for preparing a simple, green and degradable bamboo leather material according to claim 1, characterized in that: In step S1, the specific steps of preparing bamboo fiber from dried bamboo by physical or green chemical methods are as follows: the bamboo is split into two halves or pierced from the center, soaked in water, broomed three times, and then softened, fiberized, and steamed in a cooking liquid, and the degumming solution selectively removes lignin and hemicellulose, and then washed, degummed, dehydrated, and dried to obtain bamboo raw fibers.

3. The method for preparing a simple, green and degradable bamboo leather material according to claim 1, characterized in that: In step S2, the time for deionized water to dissociate the bamboo fibers is 3-6 hours.

4. The method for preparing a simple, green and degradable bamboo leather material according to claim 1, characterized in that: In step S3, the glue binding matrix liquid includes type A binding matrix and type B binding matrix, and the weight ratio of type A binding matrix to type B binding matrix is ​​1:

3.

5. The method for preparing a simple, green and degradable bamboo leather material according to claim 1, characterized in that: The solid content of the gel-binding matrix liquid is 1-5%.

6. The method for preparing a simple, green and degradable bamboo leather material according to claim 1, characterized in that: In step S3, the heating conditions are: heating for 10 min to 20 min at an initial temperature of 30°C to 60°C and a stirring speed of 0 to 1600 r / min.

7. The method for preparing a simple, green and degradable bamboo leather material according to claim 1, characterized in that: In step S5, the hot pressing conditions are: hot pressing for 10 min / mm at a temperature of 80° C. to 150° C. and a pressure of 5 KPa to 20 KPa.

8. The method for preparing a simple, green and degradable bamboo leather material according to claim 1, characterized in that: In step S3, the bamboo fiber is one or more of moso bamboo, cycad bamboo, tea stem bamboo and green bamboo.

9. The method for preparing a simple, green and degradable bamboo leather material according to claim 1, characterized in that: The weight percentage of bamboo fiber content in the prepared leather-like bamboo cellulose composite material is 20%-65%.

10. A simple, green and degradable bamboo leather material, characterized in that: The bamboo leather material is prepared by the method for preparing a simple, green and degradable bamboo leather material as described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Biodegradable composite prepreg cloth, and preparation method and device for the same

    CN103061162A

  • Modified bamboo fiber fabric and preparation method thereof

    CN109371663A

  • Preparation method for natural bamboo fiber

    CN110592685A

  • Solvent-free polylactic acid bio-based polyurethane synthetic leather, preparation method and application

    CN113699802A

  • Water-based bio-based polyurethane resin, degradable synthetic leather and preparation method of water-based bio-based polyurethane resin

    CN116284661A