Production process of easy-to-decompose non-woven cleaning cloth

Through the preparation of composite fiber layer and fiber web layer and needle-punching composite treatment, the problem of insufficient antibacterial and flexibility of existing nonwoven cleaning cloths is solved. The easily decomposed nonwoven cleaning cloths are not only good antibacterial effect, but also improved flexibility. , and is non-toxic and easy to decompose, has wide applicability, solves the problem of shatter loss and has good market prospects.

CN119061587AInactive Publication Date: 2024-12-03JIAXING SHANGYU NONWOVEN SCI TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310635201.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing disposable nonwoven cleaning cloths are insufficient in terms of antibacterial properties and flexibility, and have severe chip loss, resulting in environmental pollution problems.

Method used

The composite fiber layer and fiber web layer are prepared by cross-laying high-speed carding and hot melt blowing process to make a soft liquid-absorbing fiber web layer, and the antibacterial powder is added, and the spunbonded nonwoven fabric layer is spunbonded through needle-punching composite treatment. Combine with the composite fiber layer and finally undergo dehydration, scaling and winding to make an easy-to-decompose nonwoven cleaning cloth with antibacterial and flexible properties.

Benefits of technology

It significantly improves the antibacterial and flexibility of non-woven cleaning cloths, reduces chip loss problems, and the resulting cleaning cloth is non-toxic, easy to decompose, has a wide range of applicability, and has good market prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061587A_ABST
    Figure CN119061587A_ABST
Patent Text Reader

Abstract

The invention provides a production process of easy-to-decompose non-woven cleaning cloth, and belongs to the technical field of textile processing. According to the production process of the easily-decomposed non-woven cleaning cloth, improvement is carried out on the basis of an existing non-woven cleaning cloth production process, the product formula is optimized, the antibacterial property and flexibility of the produced non-woven cleaning cloth are remarkably improved, and the problem that traditional non-woven cleaning cloth is serious in chip falling is solved. The easy-to-decompose non-woven cleaning cloth has the advantages that the easy-to-decompose non-woven cleaning cloth is prepared by the steps of preparing the fiber web layer, preparing the non-woven cloth layer, performing needling composite treatment, dehydrating, ironing, rolling, slitting and packaging, and the easy-to-decompose non-woven cleaning cloth is simple in production process operation, is good in antibacterial effect, is flexible, non-toxic and easy to decompose, and can be widely applied to the field of cleaning and cleaning, and the production cost of the easy-to-decompose non-woven cleaning cloth is reduced. The market prospect is good, and the applicability is relatively wide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of textile processing, and in particular to a production process of an easily degradable non-woven cleaning cloth. Background Art

[0002] Nonwoven fabrics, also known as non-woven fabrics, are made of directional or random fibers. They have become a new generation of environmentally friendly materials due to their breathability, flexibility, non-toxicity, easy decomposition, and recyclability. Protective medical supplies include surgical gowns, disinfection isolation gowns, sterilization cloths, gauze, bandages, drapes, bed sheets, etc. used by medical staff. Most of them are disposable products, so the market demand is huge.

[0003] However, the inventors have found through research that in order to reduce environmental pollution, the disposable non-woven cleaning cloths currently on the market are mostly made of pulp fibers using traditional papermaking processes. Although it can meet environmental protection requirements, the product's antibacterial and flexibility are insufficient, and it sheds a lot of debris. How to invent a production process for easily degradable non-woven cleaning cloths to improve these problems has become an urgent problem to be solved by those skilled in the art. Summary of the invention

[0004] In order to make up for the above shortcomings, the present application provides a production process for an easily degradable non-woven cleaning cloth, aiming to improve the problems raised in the above background technology.

[0005] The present application embodiment provides a process for producing an easily decomposable nonwoven cleaning cloth, comprising the following steps:

[0006] Step S1, preparation of a composite fiber layer;

[0007] Step S2, preparation of a fiber web layer, forming a soft liquid-absorbent fiber web layer from cellulose fibers by a cross-lapping high-speed carding machine;

[0008] Step S3, preparation of the nonwoven fabric layer, using polylactic acid as raw material, firstly performing hot melt spraying process, then spinning the obtained hot melt spray product, and then performing drafting process, and cooling to make a gram weight of 12-28g / m 2 a spunbonded filament fiber web to obtain a nonwoven fabric layer;

[0009] Step S4, adding antibacterial powder, wherein the antibacterial powder layer is disposed between the composite fiber layer and the non-woven fabric layer;

[0010] Step S5, needle punching composite treatment, laying the nonwoven fabric layer below the composite fiber layer, and composite the spunbonded nonwoven fabric layer and the composite fiber layer into one through 4-5 needle punching processes to obtain a needle punched composite nonwoven fabric;

[0011] Step S6, dehydrating, dehydrating the obtained spunlace composite nonwoven fabric in an oven;

[0012] Step S7, ironing and rolling processing, sending the dehydrated spunlace composite nonwoven fabric into an ironing machine for ironing and then winding it into a roll to obtain a finished product;

[0013] Step S8, slitting and packaging processing, slitting the wide width coil into various narrow width coils suitable for production needs, and then packaging processing.

[0014] In a specific embodiment, in step S1, 30% bamboo pulp fiber, 40% cellulose fiber, 20% polyester fiber, and 10% ES are used to prepare a composite fiber layer according to the above mass ratio, and the cellulose fiber layer is composited into a cellulose fiber layer by a wet-laid method at a ratio of 1:8 to 5:6, and then dehydrated by negative pressure suction to obtain a 25 to 60 g / m 2 composite fiber layer.

[0015] In a specific embodiment, in the step S1, during wet web forming, the web forming speed is 100-250 m / min; the web forming slurry concentration is controlled at 2%-3%, and the output web forming curtain is subjected to negative pressure suction dehydration by a negative pressure suction fan.

[0016] In a specific embodiment, in the step S2, the operating parameters are: the speed of the cylinder roller is 850-1050 r / min, the speed of the random roller is 1020-1440 r / min, the speed of the doffer roller is 30-65 r / min, the linear speed of the output curtain is 200-300 m / min, the thickness of the fiber web of the liquid-absorbent fiber web layer is 4-15 mm, and the MD to CD strength ratio of the fiber web of the liquid-absorbent fiber web layer is less than 2.3:1.

[0017] In a specific embodiment, in step S3, a screw extruder is used to heat and melt-blow the raw materials, and the temperature of each zone of the screw extruder is controlled at 220-260°C.

[0018] In a specific embodiment, in step S3, during spinning, the temperature of the spinning box is controlled at 200-220°C; during drawing, the drawing pressure of the drawing machine is controlled at 0.1-0.3 bar, and the cooling temperature is 3-18°C.

[0019] In a specific embodiment, in step S6, the motor operation rate of the circulating fan in the oven is controlled at 55-75%, and the drying temperature is 70-100°C.

[0020] In a specific embodiment, in step S7, the temperature of the ironing machine is controlled at 110-120° C., and the winding tension of the winding machine is controlled at 0.22-0.55 bar.

[0021] Beneficial effect: The present application provides a production process for easily degradable non-woven cleaning cloth, which is an improvement on the existing production process for non-woven cleaning cloth, optimizes the product formula, and significantly improves the antibacterial property and flexibility of the produced non-woven cleaning cloth, thereby improving the serious problem of traditional non-woven cleaning cloth shedding. First, a composite fiber layer is prepared, including 30% bamboo pulp fiber, 40% cellulose fiber, 20% polyester fiber, and ES 10%, prepare the composite fiber layer according to the above mass ratio, then prepare the fiber mesh layer, make the cellulose fiber into a soft liquid-absorbing fiber mesh layer through a cross-laying high-speed carding machine, and then prepare the non-woven fabric layer by adding antibacterial powder to make the antibacterial powder layer arranged between the composite fiber layer and the non-woven fabric layer, then carry out a needle-punching composite treatment, lay the non-woven fabric layer under the composite fiber layer, and composite the spunbond non-woven fabric layer and the composite fiber layer into one through 4-5 needle-punching processes to obtain a needle-punched composite non-woven fabric, finally after dehydration, ironing and winding treatment, the dehydrated spunlace composite non-woven fabric is sent to an ironing machine for ironing and then wound into a roll to obtain a finished product, which can be shipped after slitting and packaging. The production process of the easily decomposable non-woven cleaning cloth is simple to operate, and the prepared cleaning cloth not only has good antibacterial effect, but is also flexible, non-toxic and easy to decompose, has good market prospects and is widely applicable. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the technical solutions of the implementation methods of the present application, the drawings required for use in the implementation methods will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0023] Figure 1 This is a process flow chart of the production of easily decomposable nonwoven cleaning cloth provided in the embodiment of the present application. DETAILED DESCRIPTION

[0024] The technical solutions in the embodiments of the present application will be described below in conjunction with the drawings in the embodiments of the present application.

[0025] In order to make the purpose, technical solutions and advantages of the implementation methods of this application clearer, the technical solutions in the implementation methods of this application will be clearly and completely described below in conjunction with the drawings in the implementation methods of this application. Obviously, the described implementation methods are part of the implementation methods of this application, not all of the implementation methods. Based on the implementation methods in this application, all other implementation methods obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0026] Therefore, the following detailed description of the embodiments of the present application provided in the accompanying drawings is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present application.

[0027] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.

[0028] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0029] Example 1

[0030] See also Figure 1 The present application provides a production process of a fully degradable composite nonwoven fabric for wiping, which is characterized by comprising the following steps:

[0031] Step S1, preparation of a composite fiber layer, in which 30% bamboo pulp fiber, 40% cellulose fiber, 20% polyester fiber, and 10% ES are used to prepare a composite fiber layer according to the above mass ratio, and a cellulose fiber layer is prepared by a wet-laid method at a ratio of 1:8 to 5:6, and then dehydrated by negative pressure suction to obtain a cellulose fiber layer with a gram weight of 25 to 60 g / m 2 The composite fiber layer; during the wet web forming process, the web forming speed is 100m / min; the web forming slurry concentration is controlled at 2% to 3%, and the output web forming curtain is subjected to negative pressure suction dehydration by a negative pressure suction fan;

[0032] Step S2, preparation of the fiber web layer, making the cellulose fibers into a soft liquid-absorbent fiber web layer by a cross-lapping high-speed carding machine, in which the operating parameters are: the speed of the cylinder roller is 850-1050 r / min, the speed of the random roller is 1020-1440 r / min, the speed of the doffer roller is 30-65 r / min, the linear speed of the output curtain is 200-300 m / min, the thickness of the fiber web of the liquid-absorbent fiber web layer is 4-15 mm, and the MD to CD strength ratio of the fiber web of the liquid-absorbent fiber web layer is less than 2.3:1;

[0033] Step S3, preparation of the nonwoven fabric layer, using polylactic acid and chitosan as raw materials, firstly performing a hot melt spraying process, then spinning the obtained hot melt sprayed product, and then performing a drafting process, and cooling it to make a gram weight of 12-28g / m 2 A spunbonded filament fiber web is obtained to obtain a nonwoven fabric layer; in the step S3, a screw extruder is used to heat and melt-blown the raw materials, and the temperature of each zone of the screw extruder is controlled at 220-260°C; during spinning, the temperature of the spinning box is controlled at 200-220°C; during stretching, the stretching pressure of the stretching machine is controlled at 0.1-0.3 bar, and the cooling temperature is 3-18°C;

[0034] Step S4, adding antibacterial powder, wherein the antibacterial powder layer is disposed between the composite fiber layer and the non-woven fabric layer;

[0035] Step S5, needle punching composite treatment, laying the nonwoven fabric layer below the composite fiber layer, and composite the spunbonded nonwoven fabric layer and the composite fiber layer into one through 4-5 needle punching processes to obtain a needle punched composite nonwoven fabric;

[0036] Step S6, dehydration, dehydrating the obtained spunlace composite nonwoven fabric in an oven, wherein in the step S6, the motor operation rate of the circulating fan in the oven is controlled at 55-75%; and the drying temperature is 70-100° C.;

[0037] Step S7, ironing and winding processing, sending the dehydrated spunlace composite nonwoven fabric into an ironing machine for ironing and then winding it into a roll to obtain a finished product. In the step S7, the temperature of the ironing machine is controlled at 110-120° C., and the winding tension of the winding machine is controlled at 0.22-0.55 bar;

[0038] Step S8, slitting and packaging processing, slitting the wide width coil into various narrow width coils suitable for production needs, and then packaging processing.

[0039] Example 2

[0040] See also Figure 1 The present application provides a production process of a fully degradable composite nonwoven fabric for wiping, which is characterized by comprising the following steps:

[0041] Step S1, preparation of a composite fiber layer, in which 30% bamboo pulp fiber, 40% cellulose fiber, 20% polyester fiber, and 10% ES are used to prepare a composite fiber layer according to the above mass ratio, and a cellulose fiber layer is prepared by a wet-laid method at a ratio of 1:8 to 5:6, and then dehydrated by negative pressure suction to obtain a cellulose fiber layer with a gram weight of 25 to 60 g / m 2The composite fiber layer; during the wet web forming process, the web forming speed is 175m / min; the web forming slurry concentration is controlled at 2% to 3%, and the output web forming curtain is subjected to negative pressure suction dehydration by a negative pressure suction fan;

[0042] Step S2, preparation of the fiber web layer, making the cellulose fibers into a soft liquid-absorbent fiber web layer by a cross-lapping high-speed carding machine, in which the operating parameters are: the speed of the cylinder roller is 850-1050 r / min, the speed of the random roller is 1020-1440 r / min, the speed of the doffer roller is 30-65 r / min, the linear speed of the output curtain is 200-300 m / min, the thickness of the fiber web of the liquid-absorbent fiber web layer is 4-15 mm, and the MD to CD strength ratio of the fiber web of the liquid-absorbent fiber web layer is less than 2.3:1;

[0043] Step S3, preparation of the nonwoven fabric layer, using polylactic acid and chitosan as raw materials, firstly performing a hot melt spraying process, then spinning the obtained hot melt sprayed product, and then performing a drafting process, and cooling it to make a gram weight of 12-28g / m 2 A spunbonded filament fiber web is obtained to obtain a nonwoven fabric layer; in the step S3, a screw extruder is used to heat and melt-blown the raw materials, and the temperature of each zone of the screw extruder is controlled at 220-260°C; during spinning, the temperature of the spinning box is controlled at 200-220°C; during stretching, the stretching pressure of the stretching machine is controlled at 0.1-0.3 bar, and the cooling temperature is 3-18°C;

[0044] Step S4, adding antibacterial powder, wherein the antibacterial powder layer is disposed between the composite fiber layer and the non-woven fabric layer;

[0045] Step S5, needle punching composite treatment, laying the nonwoven fabric layer below the composite fiber layer, and composite the spunbonded nonwoven fabric layer and the composite fiber layer into one through 4-5 needle punching processes to obtain a needle punched composite nonwoven fabric;

[0046] Step S6, dehydration, dehydrating the obtained spunlace composite nonwoven fabric in an oven, wherein in the step S6, the motor operation rate of the circulating fan in the oven is controlled at 55-75%; and the drying temperature is 70-100° C.;

[0047] Step S7, ironing and winding processing, sending the dehydrated spunlace composite nonwoven fabric into an ironing machine for ironing and then winding it into a roll to obtain a finished product. In the step S7, the temperature of the ironing machine is controlled at 110-120° C., and the winding tension of the winding machine is controlled at 0.22-0.55 bar;

[0048] Step S8, slitting and packaging processing, slitting the wide width coil into various narrow width coils suitable for production needs, and then packaging processing.

[0049] Example 3

[0050] See also Figure 1 The present application provides a production process of a fully degradable composite nonwoven fabric for wiping, which is characterized by comprising the following steps:

[0051] Step S1, preparation of a composite fiber layer, in which 30% bamboo pulp fiber, 40% cellulose fiber, 20% polyester fiber, and 10% ES are used to prepare a composite fiber layer according to the above mass ratio, and a cellulose fiber layer is prepared by a wet-laid method at a ratio of 1:8 to 5:6, and then dehydrated by negative pressure suction to obtain a cellulose fiber layer with a gram weight of 25 to 60 g / m 2 The composite fiber layer; during the wet web forming process, the web forming speed is 250m / min; the web forming slurry concentration is controlled at 2% to 3%, and the output web forming curtain is subjected to negative pressure suction dehydration by a negative pressure suction fan;

[0052] Step S2, preparation of the fiber web layer, making the cellulose fibers into a soft liquid-absorbent fiber web layer by a cross-lapping high-speed carding machine, in which the operating parameters are: the speed of the cylinder roller is 850-1050 r / min, the speed of the random roller is 1020-1440 r / min, the speed of the doffer roller is 30-65 r / min, the linear speed of the output curtain is 200-300 m / min, the thickness of the fiber web of the liquid-absorbent fiber web layer is 4-15 mm, and the MD to CD strength ratio of the fiber web of the liquid-absorbent fiber web layer is less than 2.3:1;

[0053] Step S3, preparation of the nonwoven fabric layer, using polylactic acid and chitosan as raw materials, firstly performing a hot melt spraying process, then spinning the obtained hot melt sprayed product, and then performing a drafting process, and cooling it to make a gram weight of 12-28g / m 2 A spunbonded filament fiber web is obtained to obtain a nonwoven fabric layer; in the step S3, a screw extruder is used to heat and melt-blown the raw materials, and the temperature of each zone of the screw extruder is controlled at 220-260°C; during spinning, the temperature of the spinning box is controlled at 200-220°C; during stretching, the stretching pressure of the stretching machine is controlled at 0.1-0.3 bar, and the cooling temperature is 3-18°C;

[0054] Step S4, adding antibacterial powder, wherein the antibacterial powder layer is disposed between the composite fiber layer and the non-woven fabric layer;

[0055] Step S5, needle punching composite treatment, laying the nonwoven fabric layer below the composite fiber layer, and composite the spunbonded nonwoven fabric layer and the composite fiber layer into one through 4-5 needle punching processes to obtain a needle punched composite nonwoven fabric;

[0056] Step S6, dehydration, dehydrating the obtained spunlace composite nonwoven fabric in an oven, wherein in the step S6, the motor operation rate of the circulating fan in the oven is controlled at 55-75%; and the drying temperature is 70-100° C.;

[0057] Step S7, ironing and winding processing, sending the dehydrated spunlace composite nonwoven fabric into an ironing machine for ironing and then winding it into a roll to obtain a finished product. In the step S7, the temperature of the ironing machine is controlled at 110-120° C., and the winding tension of the winding machine is controlled at 0.22-0.55 bar;

[0058] Step S8, slitting and packaging processing, slitting the wide width coil into various narrow width coils suitable for production needs, and then packaging processing.

[0059] The working principle of the production process of the easily degradable nonwoven cleaning cloth is as follows: First, a composite fiber layer is prepared, including 30% bamboo pulp fiber, 40% cellulose fiber, 20% polyester fiber, and ES 10%, prepare the composite fiber layer according to the above mass ratio, and then prepare the fiber mesh layer, make the cellulose fiber into a soft liquid-absorbing fiber mesh layer through a cross-laying high-speed carding machine, and then prepare the non-woven fabric layer by adding antibacterial powder to make the antibacterial powder layer arranged between the composite fiber layer and the non-woven fabric layer, and then carry out a needle-punching composite treatment, lay the non-woven fabric layer under the composite fiber layer, and composite the spunbond non-woven fabric layer and the composite fiber layer into one through 4-5 needle-punching processes to obtain a needle-punched composite non-woven fabric, and finally dehydrate, iron and roll up, send the dehydrated spunlace composite non-woven fabric into an ironing machine for ironing and then wind it into a roll to obtain the finished product, and it can be shipped out after slitting and packaging. The production process of the easily decomposable non-woven cleaning cloth is simple to operate, and the prepared cleaning cloth not only has good antibacterial effect, but is also flexible, non-toxic and easily decomposable, and has good market prospects.

[0060] The above description is only an embodiment of the present application and is not intended to limit the scope of protection of the present application. For those skilled in the art, the present application may have various changes and variations. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application should be included in the scope of protection of the present application. It should be noted that similar reference numerals and letters represent similar items in the following drawings, so once an item is defined in one drawing, it does not need to be further defined and explained in the subsequent drawings.

[0061] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A process for producing an easily degradable nonwoven cleaning cloth, characterized in that: The following steps are included: Step S1, preparation of a composite fiber layer; Step S2, preparation of a fiber web layer, forming a soft liquid-absorbent fiber web layer from cellulose fibers by a cross-lapping high-speed carding machine; Step S3, preparation of the nonwoven fabric layer, using polylactic acid as raw material, firstly performing hot melt spraying process, then spinning the obtained hot melt spray product, and then performing drafting process, and cooling to make a gram weight of 12-28g / m 2 a spunbonded filament fiber web to obtain a nonwoven fabric layer; Step S4, adding antibacterial powder, wherein the antibacterial powder layer is disposed between the composite fiber layer and the non-woven fabric layer; Step S5, needle punching composite treatment, laying the nonwoven fabric layer below the composite fiber layer, and composite the spunbonded nonwoven fabric layer and the composite fiber layer into one through 4-5 needle punching processes to obtain a needle punched composite nonwoven fabric; Step S6, dehydrating, dehydrating the obtained spunlace composite nonwoven fabric in an oven; Step S7, ironing and rolling processing, sending the dehydrated spunlace composite nonwoven fabric into an ironing machine for ironing and then winding it into a roll to obtain a finished product; Step S8, slitting and packaging processing, slitting the wide width coil into various narrow width coils suitable for production needs, and then packaging processing.

2. The process for producing an easily degradable nonwoven cleaning cloth according to claim 1, characterized in that: In step S1, 30% bamboo pulp fiber, 40% cellulose fiber, 20% polyester fiber, and 10% ES are used to prepare a composite fiber layer according to the above mass ratio, and the cellulose fiber layer is compounded by a wet-laid method in a ratio of 1:8 to 5:6, and then dehydrated by negative pressure suction to obtain a cellulose fiber layer with a gram weight of 25 to 60 g / m 2 composite fiber layer.

3. The process for producing an easily degradable nonwoven cleaning cloth according to claim 2, characterized in that: In the step S1, during wet web forming, the web forming speed is 100-250 m / min; the web forming slurry concentration is controlled at 2%-3%, and the output web forming curtain is subjected to negative pressure suction dehydration by a negative pressure suction fan.

4. The process for producing an easily degradable nonwoven cleaning cloth according to claim 1, characterized in that: In step S2, the operating parameters are: the speed of the cylinder roller is 850-1050 r / min, the speed of the random roller is 1020-1440 r / min, the speed of the doffer roller is 30-65 r / min, the linear speed of the output curtain is 200-300 m / min, the thickness of the fiber web of the liquid-absorbent fiber web layer is 4-15 mm, and the MD to CD strength ratio of the fiber web of the liquid-absorbent fiber web layer is less than 2.3:

1.

5. The process for producing an easily degradable nonwoven cleaning cloth according to claim 1, characterized in that: In the step S3, a screw extruder is used to heat and melt-blow the raw materials, and the temperature of each zone of the screw extruder is controlled at 220-260°C.

6. The process for producing an easily degradable nonwoven cleaning cloth according to claim 5, characterized in that: In the step S3, during spinning, the temperature of the spinning box is controlled at 200-220°C; during drawing, the drawing pressure of the drawing machine is controlled at 0.1-0.3 bar, and the cooling temperature is 3-18°C.

7. The process for producing an easily degradable nonwoven cleaning cloth according to claim 1, characterized in that: In step S6, the motor operation rate of the circulating fan in the oven is controlled at 55-75%, and the drying temperature is 70-100°C.

8. The process for producing an easily degradable nonwoven cleaning cloth according to claim 1, characterized in that: In step S7, the temperature of the ironing machine is controlled at 110-120° C., and the winding tension of the winding machine is controlled at 0.22-0.55 bar.