Activated carbon fiber modification method

By hydrophobic modification, impregnation modification, KI impregnation modification and flame retardant modification of activated carbon fibers, the existing nuclear power plant purifiers have solved the problems of low purification efficiency, large humidity influence and insufficient flame retardant performance, and achieved high efficiency , safe adsorption and purification effects of radioactive substances, suitable for air purification in nuclear power plants.

CN119061679APending Publication Date: 2024-12-03YANGJIANG NUCLEAR POWER +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411084360.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The iodine adsorbers used in existing nuclear power plants such as granular coconut shells or coal-based activated carbon are inefficient in purification efficiency, are susceptible to humidity, are heavy in weight and inconvenient to install, and cannot effectively adsorb radioactive substances for a long time, and their ignition point is not high, and they are flame retardant. Inadequate performance leads to insufficient purification effect and safety.

Method used

The activated carbon fiber is modified by combining hydrophobic modification, impregnation modification, KI impregnation modification and flame retardant modification, and the protective layer is formed by spraying hydrophobic solution, impregnation modification, potassium iodide impregnation and flame retardant spraying. , improve its adsorption efficiency, humidity resistance and flame retardant properties.

Benefits of technology

It significantly improves the adsorption efficiency and adsorption capacity of activated carbon fibers to radioactive substances, enhances humidity resistance and flame retardant performance, meets the requirements of nuclear-level purification, and improves the efficiency and safety of air purification in nuclear power plants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061679A_ABST
    Figure CN119061679A_ABST
Patent Text Reader

Abstract

The invention discloses an activated carbon fiber modification method which comprises the following steps: S1, spraying a mixed hydrophobic solution on activated carbon fibers, and carrying out hydrophobic modification on the activated carbon fibers, the mixed hydrophobic solution comprises tetraethoxysilane and ethanol; s2, performing impregnation modification on the activated carbon fibers; s3, dipping the activated carbon fibers in a potassium iodide aqueous solution, taking out the activated carbon fibers after a preset time, and drying the activated carbon fibers; s4, spraying the mixed flame retardant aqueous solution to the surface of the activated carbon fiber to form a flame-retardant protective layer on the surface of the activated carbon fiber; and S5, drying at a low temperature of 75-80 DEG C. According to the method for modifying the activated carbon fibers, hydrophobic modification, impregnation modification, KI impregnation modification and flame retardant modification are combined, and the activated carbon fibers are comprehensively modified, so that the performance requirements of the nuclear-grade activated carbon fibers are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nuclear power plant air purification, in particular to an activated carbon fiber modification method. Background Art

[0002] Nuclear power plants currently use iodine adsorbers based on granular coconut shells or coal-based activated carbon to purify nuclear air. Their disadvantages are: ① low purification efficiency; ② easily affected by water vapor humidity. When the humidity exceeds 80%, the purification effect drops significantly; ③ heavy weight, inconvenient to carry and install, which can easily cause purification tests to fail due to installation.

[0003] Activated carbon fiber is an activated carbon fiber, which is activated by high temperature carbonization. Its surface produces nanometer-scale pores, increasing the specific surface area, thereby changing its adsorption characteristics. Activated carbon fiber is the third generation product after powdered activated carbon and granular activated carbon. It has a large specific surface area (1000-3000m 2 / g) and abundant micropores, with the volume of micropores accounting for more than 90% of the total pore volume. Activated carbon fiber has a larger adsorption capacity and faster adsorption kinetics than granular activated carbon. It has high adsorption efficiency for organic matter and anions and cations in liquid and gas phases. It is also resistant to acid and alkali, high temperature and humidity, has strong adaptability, good conductivity and chemical stability, and is an ideal environmentally friendly purification material.

[0004] At present, the activated carbon fibers produced by factories cannot be directly used for radioactive purification in nuclear power plants. Direct use will lead to the problem of easy desorption after adsorption, that is, it cannot achieve the purpose of long-term adsorption and retention of radioactive substances. In addition, the ignition point of activated carbon fibers is not high, and the flame retardant properties need to be improved, as well as the hydrophobicity of activated carbon fibers, so as to increase the purification capacity under high humidity without significantly reducing it. Therefore, it is necessary to impregnate and modify the activated carbon fibers in order to achieve a comprehensive improvement in the purification capacity, high humidity resistance and flame retardant properties of activated carbon fibers. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a method for modifying activated carbon fibers.

[0006] The technical solution adopted by the present invention to solve the technical problem is: to provide an activated carbon fiber modification method, comprising the following steps:

[0007] S1. Spraying the activated carbon fiber with a mixed hydrophobic solution to perform hydrophobic modification on the activated carbon fiber; the mixed hydrophobic solution comprises tetraethyl orthosilicate and ethanol;

[0008] S2, impregnating and modifying the activated carbon fiber;

[0009] The impregnation material is heated and gasified, so that the impregnation material enters the micropores of the activated carbon fiber in the form of gaseous molecules;

[0010] S3, immersing the activated carbon fiber in a potassium iodide aqueous solution, taking it out after a predetermined time, and drying it;

[0011] S4, spraying the mixed flame retardant aqueous solution onto the surface of the activated carbon fiber to form a flame retardant protective layer on the surface of the activated carbon fiber;

[0012] S5. Dry at a low temperature of 75℃~80℃.

[0013] In some embodiments, in step S1, the mixed hydrophobic solution is evenly sprayed on the surface of the activated carbon fiber by a pressure spray method, and then rinsed with deionized water and dried after standing;

[0014] The mixed hydrophobic solution is prepared by preparing ethyl orthosilicate, ethanol and pure water in a molar ratio of 1:15:5.

[0015] In some embodiments, step S2 includes:

[0016] S2.1, placing the hydrophobically modified activated carbon fiber in an impregnation tank, and evacuating the impregnation tank to form a negative pressure;

[0017] S2.2, placing the impregnated material in a sealed pressure tank, heating and gasifying it and increasing the pressure in the sealed pressure tank, so that the impregnated material forms high-pressure impregnation steam;

[0018] S2.3, conveying high-pressure impregnation steam into the impregnation tank; in the impregnation tank, the high-pressure impregnation steam enters into the micropores of the activated carbon fiber.

[0019] In some embodiments, in step S2.1, after the impregnation tank is evacuated, the pressure in the impregnation tank is ≤0.99 bar.

[0020] In some embodiments, in step S2.2, the sealed pressure tank is heated so that the temperature inside reaches 200°C ± 30°C and the pressure reaches 1.6 bar to 2 bar.

[0021] In some embodiments, in step S2.2, before heating, the sealed pressure tank is purged with an inert gas to place the impregnated material under an inert gas atmosphere.

[0022] In some embodiments, the impregnant is triethylenediamine or hexamethylenetetramine.

[0023] In some embodiments, the impregnated material accounts for 10% to 15% by weight of the activated carbon fiber.

[0024] In some embodiments, step S3 includes: placing the activated carbon fiber and potassium iodide aqueous solution into a pressure vessel, and immersing the activated carbon fiber in the potassium iodide aqueous solution, and pressurizing the pressure vessel to 2 bar to 3 bar; after the activated carbon fiber is immersed in the potassium iodide aqueous solution for 10 minutes to 30 minutes, take it out and spin dry it.

[0025] In some embodiments, the concentration of the potassium iodide aqueous solution is 3% to 5%.

[0026] In some embodiments, in step S4, the mixed flame retardant aqueous solution includes sodium pyrophosphate and aluminum dihydrogen phosphate in a molar ratio of 1-1.5:2-3; the concentration of the mixed flame retardant aqueous solution is 10%-15%.

[0027] The beneficial effects of the present invention are as follows: the activated carbon fiber is comprehensively modified by combining hydrophobic modification, impregnation modification, KI impregnation modification and flame retardant modification, thereby improving the adsorption efficiency and adsorption capacity of the activated carbon fiber for radioactive substances, the humidity resistance and the flame retardant performance, and achieving the performance requirements of nuclear-grade activated carbon fiber.

[0028] The modified activated carbon fiber of the present invention can be widely used in the field of air purification in nuclear power plants, replacing traditional granular activated carbon, and bringing benefits of cost-effectiveness, reliability and safety level improvement to nuclear power plants. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The present invention will be further described below with reference to the accompanying drawings and embodiments, in which:

[0030] Figure 1 is the SEM image of activated carbon fiber before modification;

[0031] Figure 2 is a scanning electron microscope image of the activated carbon fiber modified by the present invention;

[0032] Figure 3 yes Figure 2 A partial enlarged view of

[0033] Figure 4 It adopts N 2 Pore ​​size distribution of modified activated carbon fibers measured by adsorption DFT analysis;

[0034] Figure 5 This is the pore size distribution diagram of activated carbon fiber after impregnation modification. DETAILED DESCRIPTION

[0035] The activated carbon fiber modification method of the present invention comprises the following steps:

[0036] S1. Hydrophobic modification improves the humidity resistance of activated carbon fiber.

[0037] Specifically, the activated carbon fiber is sprayed with a mixed hydrophobic solution to perform hydrophobic modification on the activated carbon fiber.

[0038] Alternatively, the mixed hydrophobic solution can be evenly sprayed on the surface of the activated carbon fiber by pressure spraying. The spraying amount is preferably enough to cover the entire surface of the activated carbon fiber without flowing out. Let it stand for more than 12 hours, then rinse with deionized water and mechanically dry it in a spin dryer.

[0039] The mixed hydrophobic solution includes tetraethyl orthosilicate and ethanol. Specifically, the mixed hydrophobic solution is prepared by preparing tetraethyl orthosilicate, ethanol and pure water in a molar ratio of 1:15:5.

[0040] S2. Impregnation modification: The hydrophobically modified activated carbon fiber is impregnated and modified.

[0041] The impregnated material is heated and gasified, so that the impregnated material enters the micropores of the activated carbon fiber in the form of gaseous molecules.

[0042] In some embodiments, step S2 may further include:

[0043] S2.1. Place the hydrophobically modified activated carbon fiber in an impregnation tank, and evacuate the tank to form a negative pressure. After the impregnation tank is evacuated, the pressure in the impregnation tank is ≤-0.99 bar.

[0044] S2.2, place the impregnated material in a sealed pressure tank, heat and vaporize it, and increase the pressure in the sealed pressure tank, so that the impregnated material forms high-pressure impregnation steam. The heating temperature is 200℃±30℃, and the pressure reaches 1.6bar~2bar.

[0045] Prior to heating, the sealed pressure vessel is purged with an inert gas (such as nitrogen) to place the impregnated material under an inert gas atmosphere.

[0046] Preferably, the impregnant is triethylenediamine or hexamethylenetetramine.

[0047] S2.3, conveying the high-pressure impregnation steam into the impregnation tank; in the impregnation tank, the high-pressure impregnation steam enters into the micropores of the activated carbon fiber.

[0048] After the high-pressure impregnation steam is delivered to the impregnation tank, the pressure inside the impregnation tank can be -0.8 to -0 bar.g.

[0049] Since the impregnation tank is in a negative pressure state, the impregnated material is heated and gasified into high-pressure impregnation steam. When the high-pressure impregnation steam is passed into the impregnation tank, the pressure difference can cause the high-pressure impregnation steam to flash explode and quickly enter the micropores of the activated carbon fiber.

[0050] In addition, by controlling the pressure in the impregnation tank or changing the initial mass of the impregnated material, impregnation modification with different mass ratios can be achieved. Preferably, the impregnation amount on the activated carbon fiber can reach 5% to 15%, that is, the mass percentage of the impregnated material to the activated carbon fiber is 5% to 15%, including 5%, 10%, 15%, etc.; within this range, the purification efficiency of the activated carbon fiber for radioactive methyl iodine can reach 99.9% or more, and the adsorption capacity is large (each gram of activated carbon fiber can adsorb more than 90 mg of methyl iodide), which meets the purification requirements of nuclear-grade activated carbon fiber.

[0051] S3, potassium iodide (KI) replacement adsorption impregnation modification.

[0052] The activated carbon fiber after step S2 is immersed in a potassium iodide aqueous solution, taken out after a predetermined time, and dried.

[0053] The specific operation of step S3 may include: placing the activated carbon fiber and the potassium iodide aqueous solution into a pressure vessel, and immersing the activated carbon fiber in the potassium iodide aqueous solution, and pressurizing the pressure vessel to 2 bar to 3 bar; after the activated carbon fiber is immersed in the potassium iodide aqueous solution for 10 minutes to 30 minutes, take it out and spin dry it.

[0054] Spin drying can be achieved by using a spin dryer.

[0055] The potassium iodide aqueous solution can be specifically formed by dissolving potassium iodide in pure water. The concentration of the potassium iodide aqueous solution is 3% to 5%.

[0056] S4, impregnation modification to improve flame retardancy.

[0057] The mixed flame retardant aqueous solution is sprayed onto the surface of the activated carbon fiber treated in step S3 by pressure spraying, and the spraying amount is preferably enough to cover the entire surface of the activated carbon fiber without flowing out. After the mixed flame retardant aqueous solution dries, a flame retardant protective layer is formed on the surface of the activated carbon fiber.

[0058] In some embodiments, the mixed flame retardant aqueous solution includes sodium pyrophosphate and aluminum dihydrogen phosphate in a molar ratio of 1 to 1.5: 2 to 3. The mixed flame retardant aqueous solution is prepared from sodium pyrophosphate, aluminum dihydrogen phosphate and pure water, and the concentration of the mixed flame retardant aqueous solution is 10% to 15%.

[0059] S5. Dry at a low temperature of 75℃~80℃.

[0060] Specifically, the activated carbon fiber modified by the above steps S1 to S4 is placed in a drying oven and dried at a temperature of 75° C. to 80° C. for 2 to 3 hours to obtain dried modified activated carbon fiber.

[0061] (I) Methyl iodide removal test:

[0062] The test was carried out according to ASTM D3803-1991. Specifically, the modified activated carbon fiber was tested in the form of an adsorption bed, and the specific conditions are shown in Table 1 below.

[0063] Table 1

[0064]

[0065] Test results: adsorption efficiency 99.909% ± 0.012%;

[0066] Penetration efficiency 0.091%±0.012%.

[0067] It can be seen from the above test results that at 85% humidity, the purification efficiency of the modified activated carbon fiber for methyl iodide is higher than 99.9%.

[0068] (II) Purification capacity and life test:

[0069] The test conditions and results are shown in Table 2 below.

[0070] Table 2

[0071]

[0072]

[0073] It can be seen from Table 2 above that the adsorption and purification capacity of the modified activated carbon fiber is greatly improved. Each gram of activated carbon fiber can adsorb more than 94 mg of radioactive methyl iodide, which is far more than 8 mg of radioactive methyl iodide adsorbed by each gram of granular activated carbon, thereby greatly improving the service life of the filter made of activated carbon fiber.

[0074] (III) Flame retardant performance test:

[0075] The flame retardant performance results are shown in Table 3 below.

[0076] Table 3

[0077]

[0078] From the above results, it can be seen that the flame retardant properties of the activated carbon fiber modified by flame retardant impregnation are greatly improved, and the ignition point is increased to above 420°C, which is much higher than the 280°C of granular activated carbon. In addition, the modified activated carbon fiber has very little combustible part, avoiding the risk of fire.

[0079] The activated carbon fiber modified by the present invention has a smooth surface before and after modification, respectively. Figure 1 and Figure 2 As shown. Figure 2 and Figure 3From the scanning electron microscope image, it can be seen that the activated carbon fiber filaments modified by the present invention have a smooth appearance, no residual crystals of the impregnated material, the impregnated material enters the interior of the activated carbon fiber filaments or is evenly distributed on the outer surface, and there is no accumulation and clogging of the micropores.

[0080] Using N 2 The adsorption DFT analysis method was used to measure the pore size distribution of activated carbon fibers before and after modification. Figure 4 As shown. Figure 4 It can be seen that the pore structure of the modified activated carbon fiber is mainly micropores, pores smaller than 2nm account for 98% of the total pores, and the average pore diameter is 1.65nm.

[0081] According to the van der Waals adsorption theory, when the pore size of the adsorbent is 1.5 to 2 times the size of the adsorbate, the adsorbate molecules can effectively accept the adsorption force field superimposed on the micropore surface, which is most conducive to the adsorption of the adsorbate. The average pore size of the modified activated carbon fiber is 1.65nm, which is larger than the diameter of methyl iodide molecules of 0.5nm, so it is conducive to the adsorption of methyl iodide.

[0082] The impregnation modification of activated carbon fiber allows the modified impregnant to enter the micropores, thereby reducing the pore size to a certain extent, which indirectly plays a role in regulating the pore size. In order to evaluate this regulation effect, the pore size test of the impregnated modified activated carbon fiber was performed again. The results are as follows Figure 5 .Depend on Figure 5 It can be seen that the average pore size of the activated carbon fiber after impregnation modification is 1.01 nm, which is twice the diameter of the methyl iodide molecule, which is conducive to physical adsorption.

[0083] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for modifying activated carbon fiber, It is characterized in that The following steps are involved: S1. Spraying the activated carbon fiber with a mixed hydrophobic solution to perform hydrophobic modification on the activated carbon fiber; the mixed hydrophobic solution comprises tetraethyl orthosilicate and ethanol; S2, impregnating and modifying the activated carbon fiber; The impregnation material is heated and gasified, so that the impregnation material enters the micropores of the activated carbon fiber in the form of gaseous molecules; S3, immersing the activated carbon fiber in a potassium iodide aqueous solution, taking it out after a predetermined time, and drying it; S4, spraying the mixed flame retardant aqueous solution onto the surface of the activated carbon fiber to form a flame retardant protective layer on the surface of the activated carbon fiber; S5. Dry at a low temperature of 75℃~80℃.

2. The activated carbon fiber modification method according to claim 1, It is characterized in that In step S1, the mixed hydrophobic solution is uniformly sprayed on the surface of the activated carbon fiber by a pressure spray method, and after standing, it is rinsed with deionized water and dried; The mixed hydrophobic solution is prepared by preparing ethyl orthosilicate, ethanol and pure water in a molar ratio of 1:15:

5.

3. The method for modifying activated carbon fiber according to claim 1, It is characterized in that Step S2 includes: S2.1, placing the hydrophobically modified activated carbon fiber in an impregnation tank, and evacuating the impregnation tank to form a negative pressure; S2.2, placing the impregnated material in a sealed pressure tank, heating and gasifying it and increasing the pressure in the sealed pressure tank, so that the impregnated material forms high-pressure impregnation steam; S2.3, conveying high-pressure impregnation steam into the impregnation tank; in the impregnation tank, the high-pressure impregnation steam enters into the micropores of the activated carbon fiber.

4. The method for modifying activated carbon fiber according to claim 3, It is characterized in that In step S2.1, after the impregnation tank is evacuated, the pressure in the impregnation tank is ≤0.99 bar; In step S2.2, the sealed pressure tank is heated so that the temperature inside reaches 200°C ± 30°C and the pressure reaches 1.6 bar to 2 bar.

5. The method for modifying activated carbon fiber according to claim 3, It is characterized in that In step S2.2, before heating, the sealed pressure tank is purged with an inert gas to place the impregnated material under an inert gas atmosphere.

6. The method for modifying activated carbon fiber according to any one of claims 1 to 5, It is characterized in that The impregnated material is triethylenediamine or hexamethylenetetramine.

7. The method for modifying activated carbon fiber according to any one of claims 1 to 5, It is characterized in that The mass percentage of the impregnated material to the activated carbon fiber is 10% to 15%.

8. The method for modifying activated carbon fiber according to any one of claims 1 to 5, It is characterized in that Step S3 comprises: placing the activated carbon fiber and the potassium iodide aqueous solution into a pressure vessel, immersing the activated carbon fiber in the potassium iodide aqueous solution, and pressurizing the pressure vessel to 2 bar to 3 bar; The activated carbon fibers are taken out after being immersed in the potassium iodide aqueous solution for 10 to 30 minutes and then dried.

9. The method for modifying activated carbon fiber according to any one of claims 1 to 5, It is characterized in that The concentration of the potassium iodide aqueous solution is 3% to 5%.

10. The method for modifying activated carbon fiber according to any one of claims 1 to 5, It is characterized in that In step S4, the mixed flame retardant aqueous solution includes sodium pyrophosphate and aluminum dihydrogen phosphate in a molar ratio of 1-1.5:2-3; the concentration of the mixed flame retardant aqueous solution is 10%-15%.