Preparation process of pelelith composite material and moisture absorption and sweat releasing cloth
After mixing volcanic stone with powder particles and forming in a polymer substrate, cleaning with acidic liquid to restore the porous structure, the problem of blockage of the porous structure of the volcanic stone is solved, and the moisture absorption and breathability performance is significantly improved.
Patent Information
- Application Number
- CN202410998329.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-07-24
Smart Images

Figure CN119061683A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite materials and relates to a preparation process of a volcanic rock composite material and a moisture absorbing and perspiration wicking fabric. Background Art
[0002] Volcanic rock is a functional and environmentally friendly material. It is a porous stone formed by volcanic glass, minerals and bubbles after a volcanic eruption. Volcanic rock contains dozens of minerals and trace elements such as sodium, magnesium, aluminum, silicon, calcium, titanium, manganese, iron, nickel, cobalt and molybdenum. It has functions such as ultraviolet reflection. The yarn and fabric surface structure added and made are porous, which not only has good water absorption and strong moisture absorption and perspiration function, but also has a certain ultraviolet reflection function, and can deepen the color and reduce the addition of dyes.
[0003] In the prior art, volcanic rocks are generally prepared into masterbatches directly or after surface modification, and then added to polymer materials to prepare yarns or fibers. This leads to a problem that the masterbatch material or polymer material easily enters the porous structure of the volcanic rocks, causing the porous structure of the volcanic rocks to be partially or completely blocked, making it impossible to exert the porous characteristics and functions of the volcanic rocks, and affecting the moisture absorption and perspiration function of the fabric.
[0004] Therefore, it is urgent to solve the above problems. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a preparation process of a volcanic rock composite material and a moisture absorbing and perspiration-releasing fabric.
[0006] The technical solution of the present invention is as follows:
[0007] A preparation process of a volcanic rock composite material comprises the following steps:
[0008] mixing the volcanic rock and the powder particles to obtain a premix;
[0009] Dispersing the premix into a polymer matrix and forming the preform to obtain a preform;
[0010] The preform is washed with an acidic liquid to obtain the volcanic stone composite material;
[0011] The powder particles and the acidic aqueous solution may react at 100° C. or less, and a reaction product may be dissolved in the acidic aqueous solution.
[0012] Preferably, the average particle size of the volcanic rock is 1-30 μm.
[0013] Preferably, the powder particles are selected from one or a combination of two or more of carbonates, bicarbonates, metal hydroxides and metal oxides.
[0014] Preferably, the weight ratio of the volcanic rock to the powder particles is 20:1-1:10.
[0015] Preferably, the weight ratio of the premix to the polymer substrate is 3-40:100.
[0016] Preferably, the dispersing method is selected from bulk blending and solution blending.
[0017] Preferably, the polymer substrate is selected from one or a combination of two or more of natural polymers and synthetic polymers.
[0018] Preferably, the pH of the acidic liquid is no more than 4.
[0019] A moisture absorbing and perspiration-releasing fabric is prepared by the preparation process of the volcanic rock composite material described in any one of the above embodiments.
[0020] Preferably, the preform is first prepared into an initial cloth, and then washed with an acidic aqueous solution to obtain the cloth;
[0021] Alternatively, the volcanic rock composite material is obtained and then prepared into the cloth.
[0022] The beneficial effects of the present invention are:
[0023] (1) The present invention pre-treats and seals the porous structure of volcanic rock with powder particles. During the molding process of the treated volcanic rock, the polymer matrix cannot penetrate into the porous structure. After the composite material of the volcanic rock and the polymer matrix is molded, the powder particles are reacted with an acidic liquid. The reaction product of the powder particles dissolves in the acidic liquid, thereby restoring the porous structure of the volcanic rock.
[0024] (2) The process of the present invention is simple and has good effects. The porous structure of the volcanic stone can be fully utilized to prepare fabrics with good moisture absorption and perspiration removal effects. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the SEM image of the volcanic rock composite fiber in Example 1.
[0026] Figure 2 This is the SEM image of the preformed fiber in Example 1. DETAILED DESCRIPTION
[0027] The technical solution of the present invention is further illustrated and described below through specific implementation methods.
[0028] In order to solve the problem that the porous structure of the volcanic stone is blocked by the polymer matrix after the volcanic stone and the polymer matrix form a composite material, on the one hand, the present invention provides a preparation process of the volcanic stone composite material, comprising the following steps:
[0029] mixing the volcanic rock and the powder particles to obtain a premix;
[0030] Dispersing the premix into a polymer matrix and forming the preform to obtain a preform;
[0031] The preform is washed with an acidic liquid to obtain a volcanic stone composite material;
[0032] The powder particles and the acidic aqueous solution may react at 100° C. or below, and the reaction product may be dissolved in the acidic aqueous solution.
[0033] For example, taking the preparation of preforms by melt extrusion molding as an example, the operation method can be as follows: (1) drying each raw material component; (2) weighing each raw material component after drying according to the formula; (3) mixing the premix and the polymer matrix (or other raw material components, such as antioxidants, dispersants, etc.) into a mixer, stirring for 15 to 30 minutes at a stirring rate of 100 to 150 r / min; (4) adding the above mixture to a twin-screw extruder, melt extrusion granulation or direct molding, and then drying. The twin-screw extruder can adopt 11-zone temperature settings. For example, for PET resin, the set temperatures are 150-160°C, 230-240°C, 240-250°C, 250-260°C, 250-260°C, 220-230°C, 220-230°C, 220-230°C, 220-230°C, 220-230°C, 240-250°C. The cooling temperature is 15-30°C. The screw speed of the twin-screw extruder is set to 300-500r / min. If melt extrusion granulation is used, the obtained masterbatch can be added to conventional chemical fiber polymers for melt spinning molding.
[0034] The present invention uses powder particles to block the porous structure of volcanic rocks in advance, and then mixes with a polymer substrate and forms molding materials such as fibers, particles, plates, etc. The polymer substrate cannot enter the porous structure of the volcanic rocks. Then, an acidic solution reacts with the powder particles on the surface of the molding materials (fibers, particles, plates, films, etc.), and the reaction product dissolves in the acidic liquid. As the acidic solution gradually penetrates, the blocking powder particles of the volcanic rocks from the outside to the inside of the molding materials are gradually reacted and dissolved. The acidic solution can penetrate into the porous structure of the volcanic rocks inside the molding materials and react with the powder particles. The product dissolves in the acidic solution, and the porous structure of the volcanic rocks is restored, so that the volcanic rocks of the obtained volcanic rock composite material have their original porous structure, and the characteristics of the volcanic rocks are brought into play. The volcanic rock composite material has good moisture absorption and air permeability functions.
[0035] Specifically, there is no particular limitation on the method of preparing a premix by mixing volcanic rocks and powder particles. One method may be as follows: volcanic rocks and powder particles are mixed and vibrated using a vibrating screen (e.g., the screen may be 300-500 meshes) to obtain a premix, which can not only promote the clogging of the porous structure of the volcanic rocks by the powder particles, but also remove excess powder particles to prevent the excess powder particles from being adsorbed on the surface of the volcanic rocks, and then when mixed with the polymer matrix, the powder particles remain on the polymer matrix. Alternatively, further, the pretreated volcanic rocks are soaked in water for a certain period of time (e.g., 1-30 minutes) to remove the powder particles on the surface of the volcanic rocks, and the powder particles filled in the porous structure of the volcanic rocks still exist, and then the volcanic rocks are separated and dried to obtain the premix.
[0036] In a preferred embodiment of the present invention, the average particle size of the volcanic stone is 1-30 μm. If the average particle size of the volcanic stone is too low, it is easy to agglomerate and the moisture absorption and air permeability are poor. If the average particle size of the volcanic stone is too large, it will affect the mechanical properties of the volcanic stone composite material. Those skilled in the art know that the average particle size of the volcanic stone can be different for different molding materials. For example, for fibers, the average particle size of the volcanic stone can be 1-10 μm, or further, 1-5 μm; for plates, the average particle size of the volcanic stone can be 10-30 μm. Specifically, the average particle size of the volcanic rock can be any value among 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm, 20μm, 21μm, 22μm, 23μm, 24μm, 25μm, 26μm, 27μm, 28μm, 29μm, 30μm, etc., but is not limited to the above-mentioned values.
[0037] In a preferred embodiment of the present invention, the powder particles are selected from one or a combination of two or more of carbonates, bicarbonates, metal hydroxides and metal oxides. The above powder particles can react with an acidic solution at 100°C or below, and the reaction product dissolves in the acidic solution, so that the porous structure of the volcanic rock that is blocked restores its porous properties. For example, carbonates can be sodium carbonate, potassium carbonate, magnesium carbonate, calcium carbonate, lithium carbonate, zinc carbonate, ammonium carbonate, etc., bicarbonates can be sodium bicarbonate, potassium bicarbonate, magnesium bicarbonate, ammonium bicarbonate, etc., metal hydroxides can be sodium hydroxide, potassium hydroxide, lithium hydroxide, calcium hydroxide, magnesium hydroxide, aluminum hydroxide, barium hydroxide, zinc hydroxide, etc., and metal oxides can be calcium oxide, magnesium oxide, zinc oxide, lithium oxide, barium oxide, etc. In the present invention, the powder particles can be nanometer-sized, such as 10nm-500nm, so as to facilitate the powder particles to enter the porous structure of the volcanic rock.
[0038] In a preferred embodiment of the present invention, the weight ratio of volcanic rock to powder particles is 20:1-1:10. When the weight ratio of volcanic rock to powder particles is within the above range, the powder particles are excessive or just relative to the volcanic rock, and the porous structure of the volcanic rock can be blocked well. For example, the weight ratio of volcanic rock to powder particles can be any value of 20:1, 18:1, 16:1, 15:1, 12:1, 10:1, 8:1, 6:1, 5:1, 4:1, 3:1, 2:1, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, etc., but is not limited to the above.
[0039] In a preferred embodiment of the present invention, the weight ratio of the premix to the polymer matrix is 3-40:100. When the weight ratio of the premix to the polymer matrix is within the above range, the moisture absorption and breathability of the volcanic stone can be better exerted. For example, the weight ratio of the premix to the polymer matrix can be 3:100, 4:100, 5:100, 6:100, 7:100, 8:100, 9:100, 10:100, 11:100, 12:100, 13:100, 14:100, 15:100, 16:100, 17:100, 18:100, 19:100, 20:100, 21:100, 22:100, 23:100, 24:100, 25:100, 26:100, 27:100, 28:100, 29:100, 30:100, 31:100, 32:100, 33:100, 34:100, 35:100, 36:100, 37:100, 38:100, 39:100, 40:100, 41:100, 42:100, 43:100, 44:100 Any value among 2:100, 23:100, 24:100, 25:100, 26:100, 27:100, 28:100, 29:100, 30:100, 31:100, 32:100, 33:100, 34:100, 35:100, 36:100, 37:100, 38:100, 39:100, 40:100, etc., but not limited to the above-mentioned values.
[0040] In a preferred embodiment of the present invention, the dispersion method is selected from bulk blending and solution blending. Bulk blending refers to blending volcanic rock (or volcanic rock pre-made into volcanic rock masterbatch) with polymer bulk. Based on the properties of the polymer bulk, bulk blending can be divided into melt blending and room temperature blending. For polymer materials that are solid at room temperature, such as polyethylene, polypropylene, polyurethane, etc., melt blending can be used. Melt blending is to mix volcanic rock directly with the polymer matrix, and then heat the polymer matrix to melt. The volcanic rock and the liquid polymer matrix are mixed by the shearing action of external force, or the volcanic rock can be prepared into a masterbatch with part of the polymer matrix in advance, and then mixed with the remaining polymer matrix. The molding after melt blending can be extrusion molding, injection molding, compression molding, etc., and the molded profile can be in the form of fiber, film, plate, granule, etc.; For polymer materials that are in a rubber state at room temperature, such as polysiloxane, nitrile rubber, EPDM rubber, etc., room temperature blending can be used to disperse the volcanic rock into the polymer material by external forces such as screw shearing, or it can continue to be cured with a curing agent at a certain temperature. The molding after room temperature blending can be extrusion molding, injection molding, compression molding, etc., and a curing agent or a cross-linking agent can be added for further cross-linking and curing. Solution blending can be a process of mixing a polymer substrate with a solvent (water or an organic solvent) to form a polymer solution, adding volcanic rock and mixing through the shearing action of an external force, and then forming the solution solution by solution spinning, cast film, etc. The formed profile can be in the form of fibers, films, etc.
[0041] The preparation process of the volcanic rock composite material of the present invention has no particular restrictions on the polymer substrate. In a preferred embodiment of the present invention, the polymer substrate is selected from one or a combination of two or more of natural polymers and synthetic polymers. For example, the natural polymer can be cotton fiber, hemp fiber, wool fiber, silk fiber; the synthetic polymer can be polyethylene, polypropylene, polyurethane, polyester, acrylic resin, epoxy resin, polyurea, nylon, polyvinyl chloride, polyacrylonitrile, polystyrene, etc.
[0042] In a preferred embodiment of the present invention, the pH of the acidic liquid does not exceed 4. The acidic solution of the present invention can be an organic acid or an inorganic acid, and can also be a pure acid or an acidic aqueous solution. For organic acids, such as acetic acid, malic acid, citric acid, oxalic acid, tartaric acid, methanesulfonic acid, trifluoromethanesulfonic acid, benzoic acid, benzenesulfonic acid, toluenesulfonic acid, etc., it can be a pure acid or an acidic aqueous solution, and the concentration of the acidic aqueous solution can be 0.01-10mol / L, such as 0.01mol / L, 0.1mol / L, 0.3mol / L, 0.5mol / L, 1mol / L, 2mol / L, 3mol / L, 4mol / L, 5mol / L, etc., any value, but not limited to the above listed. For inorganic acid, it can be an inorganic acid aqueous solution, such as hydrochloric acid solution, sulfuric acid solution, nitric acid solution, phosphoric acid solution, etc., and the concentration can be 0.01-3mol / L, such as 0.01mol / L, 0.1mol / L, 0.3mol / L, 0.5mol / L, 1mol / L, 1.5mol / L, 2mol / L, 2.5mol / L, 3mol / L, etc., but not limited to the above. The pH of the acidic liquid does not exceed 4, and it can react with the powder particles faster. Further, the pH of the acidic liquid does not exceed 3. For example, the pH can be any value of 3, 2.8, 2.5, 2.3, 2.2, 2, 1.8, 1.6, 1.5, 1.2, 1, 0.8, 0.5, 0.3, 0.2, 0, etc., but not limited to the above.
[0043] On the other hand, the present invention provides a moisture wicking fabric, which is prepared by the preparation process of the volcanic rock composite material described in any of the above embodiments. The above polymer substrate is selected as a material commonly used for fabrics, such as synthetic polypropylene, aramid, spandex, polyester, nylon, acrylic, etc., and natural cotton, linen, etc., to prepare a fabric with moisture wicking function. In addition to volcanic rock and polymer substrate, the fabric may also contain antioxidants, antistatic agents, anti-ultraviolet agents, dispersants, dyes, etc., which can be further screened and used according to the specific functions of the fabric.
[0044] In a preferred embodiment of the present invention, the preform is first prepared into an initial cloth, and then washed with an acidic aqueous solution to obtain the cloth;
[0045] Or, the volcanic rock composite material is obtained and then prepared into cloth.
[0046] By adopting the above two preparation methods, the volcanic rock composite material can be prepared by the present invention and further prepared into a fabric with moisture absorption and perspiration discharge function.
[0047] The technical solution of the present invention is further described and illustrated according to various embodiments below. Unless otherwise specified, the parts described in the following embodiments are parts by weight.
[0048] Example 1
[0049] 20 parts of volcanic rock with an average particle size of 3 μm and 1 part of sodium carbonate with an average particle size of 80 nm were mixed in a three-dimensional mixer for 10 minutes, and then transferred to a 500-mesh vibrating sieve for sieving to obtain a premix;
[0050] The PET polyester raw material was pre-dried. 10 parts of the above premix and 100 parts of PET polyester were mixed and added into a twin-screw extruder to extrude and form fibers (diameter 0.5 mm) to obtain preformed fibers.
[0051] The preformed fibers were immersed in an acetic acid solution (10 wt % concentration) and ultrasonically cleaned for 5 min, taken out, ultrasonically cleaned twice with clean water, and dried at 60° C. overnight to obtain volcanic rock composite fibers.
[0052] In the present invention, the SEM picture of the volcanic rock composite fiber is as shown in the attached Figure 1 As shown in the figure, it can be seen that the surface of the volcanic rock composite fiber has a rich porous structure; the SEM image of the above preformed fiber is shown in the attached Figure 2 As shown, the surface of the fiber is covered with polypropylene, and the porous structure of the volcanic stone is basically invisible.
[0053] Therefore, the preparation process of the present invention can prevent the porous structure of the volcanic stone from being blocked by the polymer substrate, maintain the porous structure of the volcanic stone, and enable the volcanic stone composite fiber to exert the characteristics of the volcanic stone and have good absorption and ventilation effects.
[0054] Example 2
[0055] The difference between Example 2 and Example 1 is that in Example 1, 20 parts of volcanic rock with an average particle size of 3 μm is adjusted to 14 parts, and 1 part of sodium carbonate with an average particle size of 80 nm is adjusted to 7 parts. The remaining steps remain unchanged.
[0056] Example 3
[0057] The difference between Example 3 and Example 1 is that in Example 1, 20 parts of volcanic rock with an average particle size of 3 μm is adjusted to 10 parts, and 1 part of sodium carbonate with an average particle size of 80 nm is adjusted to 11 parts. The other steps remain unchanged.
[0058] Example 4
[0059] The difference between Example 4 and Example 1 is that in Example 1, 20 parts of volcanic rock with an average particle size of 3 μm is adjusted to 2 parts, and 1 part of sodium carbonate with an average particle size of 80 nm is adjusted to 19 parts. The remaining steps remain unchanged.
[0060] Comparative Example 1
[0061] The preformed fiber in Example 1.
[0062] Comparative Example 2
[0063] 10 parts of the untreated volcanic rock in Example 1 and 100 parts of the PET polyester in Example 1 were mixed, added into a twin-screw extruder and extruded into fibers (diameter 0.5 mm), to obtain volcanic rock composite fibers.
[0064] Comparative Example 3
[0065] The difference between Comparative Example 3 and Comparative Example 2 is that in Comparative Example 2, the weight of the untreated volcanic rock is adjusted from 10 parts to 0 parts. The remaining steps remain unchanged.
[0066] Comparative Example 4
[0067] The difference between Comparative Example 4 and Comparative Example 2 is that in Comparative Example 2, the weight of the untreated volcanic rock is adjusted from 10 parts to 20 parts. The remaining steps remain unchanged.
[0068] Example 5
[0069] 10 parts of volcanic rock with an average particle size of 5 μm and 10 parts of sodium bicarbonate with an average particle size of 200 nm were mixed in a three-dimensional mixer for 10 minutes, transferred to a 500-mesh vibrating screen for sieving, the sieved treated volcanic rock was added to 100 parts of water, stirred for 3 minutes, filtered, and the filtered solid was dried at 100° C. for 6 hours to obtain a premix.
[0070] 3 parts of the above premix and 100 parts of PET polyester were mixed, added into a twin-screw extruder and extruded into fibers (1 mm in diameter) to obtain preformed fibers;
[0071] The preformed fibers were immersed in a sulfuric acid solution with a concentration of 0.1 mol / L for 2 minutes, taken out, ultrasonically cleaned with clean water for 3 times, and dried at 60° C. overnight to obtain volcanic rock composite fibers.
[0072] Example 6
[0073] The difference between Example 6 and Example 5 is that in Example 5, the premix is adjusted from 3 parts to 10 parts. The other steps remain unchanged.
[0074] Example 7
[0075] The difference between Example 7 and Example 5 is that in Example 5, the premix is adjusted from 3 parts to 20 parts. The other steps remain unchanged.
[0076] Example 8
[0077] The difference between Example 8 and Example 5 is that in Example 5, the premix is adjusted from 3 parts to 40 parts. The other steps remain unchanged.
[0078] The drying speed, wick height, water absorption rate and drip diffusion time were tested according to the method of GB / T 21655.1-2023. The results are shown in Table 1. The faster the drying speed, the larger the wick height, the higher the water absorption rate and the shorter the drip diffusion time, the better the moisture absorption and air permeability.
[0079] Table 1
[0080]
[0081] Comparing the data results in Table 1 above, it can be seen from Examples 1-4 that changing the ratio of volcanic rock to powder particles has no significant effect on the water absorption and air permeability of the volcanic rock composite fiber. The reason is that as long as the porous structure of the volcanic rock is fully blocked, and then the powder particles are fully removed with an acidic solution, the porous structure is restored and the effect is exerted. Comparing Examples 1-4, Comparative Example 2, Comparative Example 4 and Comparative Example 3, adding untreated volcanic rock can improve the water absorption and air permeability, but the effect is not very obvious. If the porous structure is blocked and not cleaned and removed, it cannot exert the effect of water absorption and air permeability. Comparing Examples 5-8, as the amount of volcanic rock increases, the air permeability and hygroscopicity become better and better.
[0082] Example 9
[0083] 10 parts of volcanic rock with an average particle size of 10 μm and 10 parts of sodium bicarbonate with an average particle size of 500 nm were mixed in a three-dimensional mixer for 10 minutes, transferred to a 500-mesh vibrating screen for sieving, the sieved treated volcanic rock was added to 100 parts of water, stirred for 3 minutes, filtered, and the filtered solid was dried at 100° C. for 6 hours to obtain a premix.
[0084] 15 parts of the above premix, 100 parts of polyurethane elastomer TPU, 0.5 parts of antioxidant 1010, 0.6 parts of UV-327 and 1 part of KH-560 coupling agent were mixed, added into a mixer for mixing, and then prepared into a preformed plate with a size of 10 cm×10 cm×2 mm by a compression molding method;
[0085] The preformed plate was immersed in an oxalic acid solution with a concentration of 0.1 mol / L and ultrasonically cleaned for 10 min. The preformed plate was taken out, ultrasonically cleaned with clean water for 3 times, and dried at 60° C. overnight to obtain a volcanic stone composite plate.
[0086] Example 10
[0087] The difference between Example 10 and Example 9 is that in Example 9, the average particle size of the volcanic rock is adjusted from 10 μm to 30 μm. The other steps remain unchanged.
[0088] Comparative Example 5
[0089] The difference between Comparative Example 5 and Example 9 is that in Example 9, the premix is replaced by an equal weight of untreated volcanic rock (in Example 9). The remaining steps remain unchanged.
[0090] Comparative Example 6
[0091] 100 parts of the polyurethane elastomer TPU in Example 9, 0.5 parts of antioxidant 1010, 0.6 parts of UV-327 and 1 part of KH-560 coupling agent were mixed, added to a mixer for mixing, and then prepared into a polyurethane sheet with a size of 10 cm×10 cm×2 mm by a compression molding method.
[0092] According to the method of GB / T 21655.1-2023, the drip diffusion time of the plates of Example 9, Example 10, Comparative Example 5 and Comparative Example 6 was 2.1s, 1.8s, 4.9s and 5.5s respectively, and the drying speed was 0.38g / h, 0.41g / h, 0.20g / h and 0.17g / h respectively. Therefore, the process method of the present invention can significantly improve the moisture absorption and air permeability of the volcanic stone composite material.
[0093] As described above, the basic principles, main features and advantages of the present invention are shown and described. Those skilled in the art should understand that the present invention is not limited by the above embodiments, which are only preferred embodiments of the present invention and cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the scope of the present invention and the content of the specification should still be within the scope of the present invention. The scope of protection required by the present invention is defined by the attached claims and their equivalents.
Claims
1. A process for preparing a volcanic rock composite material, characterized in that: The following steps are involved: mixing the volcanic rock and the powder particles to obtain a premix; Dispersing the premix into a polymer matrix and forming the preform to obtain a preform; The preform is washed with an acidic liquid to obtain the volcanic stone composite material; The powder particles and the acidic aqueous solution may react at 100° C. or less, and a reaction product may be dissolved in the acidic aqueous solution.
2. The process for preparing the volcanic rock composite material according to claim 1, characterized in that: The average particle size of the volcanic rock is 1-30 μm.
3. The process for preparing the volcanic rock composite material according to claim 1, characterized in that: The powder particles are selected from one or a combination of two or more of carbonates, bicarbonates, metal hydroxides and metal oxides.
4. The process for preparing the volcanic rock composite material according to claim 1, characterized in that: The weight ratio of the volcanic rock to the powder particles is 20:1-1:
10.
5. The process for preparing the volcanic rock composite material according to claim 1, characterized in that: The weight ratio of the premix to the polymer matrix is 3-40:
100.
6. The process for preparing the volcanic rock composite material according to claim 1, characterized in that: The dispersing method is selected from bulk blending and solution blending.
7. The process for preparing the volcanic rock composite material according to claim 1, characterized in that: The polymer substrate is selected from one or a combination of two or more of natural polymers and synthetic polymers.
8. The process for preparing the volcanic rock composite material according to claim 1, characterized in that: The pH of the acidic liquid does not exceed 4.
9. A moisture wicking fabric, characterized in that: The volcanic rock composite material is prepared by the preparation process of any one of claims 1 to 8.
10. The moisture wicking fabric according to claim 9, characterized in that: The preform is first prepared into an initial cloth, and then washed with an acidic aqueous solution to obtain the cloth; Alternatively, the volcanic rock composite material is obtained and then prepared into the cloth.
Citation Information
Patent Citations
Knitted fabric containing volcanic ash microcrystal particles and preparation method thereof
CN102260954A
Method for producing antimicrobial polyester fiber yarn containing volcanic ash
CN106958049A
Preparation method of rare earth element modified heat-resistant textile
CN108385392A
Moisture-absorbing quick-dry light fiber with honeycomb structure and preparation method thereof
CN118272951A
Solvent-free production of porous polymer structures
US20220410075A1