Moisture-absorbing and sweat-releasing breathable fabric and preparation method thereof
Through the blending of acrylic fiber, viscose fiber, spandex fiber and cuproammonia fiber, combined with wool fiber, the problem of existing fabrics being difficult to take into account moisture absorption, sweating, breathability and warmth, and the wear resistance and elasticity of the fabric are improved. For multi-functional clothing.
Patent Information
- Application Number
- CN202411144250.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-20
AI Technical Summary
Existing functional fabrics are difficult to take into account both moisture-wicking, breathable and warmth, and are not wear-resistant and deformable, which affects the comfort of wearing.
Breathable fabrics made of acrylic fibers, viscose fibers, spandex fibers and cuproamino fibers are used to blend and knitize with wool fibers. The cuproamino fibers are pretreated to improve their dispersion and fluffyness, forming fabrics and linings that fit the structure. , optimize fiber ratio to improve elasticity and wear resistance.
The prepared breathable fabric has moisture absorption, breathability, warmth, elasticity and non-deformability. It is suitable for different climatic conditions and has a wide range of applications. It is suitable for close-fitting clothing fabrics.
Smart Images

Figure BDA0005001783240000051 
Figure BDA0005001783240000061 
Figure BDA0005001783240000071
Abstract
Description
Technical Field
[0001] The present application relates to the field of functional fabrics, and more specifically, to a moisture absorbing and perspiration wicking breathable fabric and a preparation method thereof. Background Art
[0002] As people's quality of life continues to improve, the demand for the texture and comfort of clothing is also getting higher and higher. The comfort of wearing clothes comes from the fabrics used for clothing. In order to adapt to different climates and temperatures, the fabrics need to have multiple properties. For example: in the hot summer, when the temperature is high, the fabrics need to have the functions of moisture absorption and perspiration and breathability, while in the cold winter, when the temperature is low and the skin is prone to dryness, the fabrics need to have better warmth retention, breathability and anti-static properties, and the above fabrics need to have good wear resistance and non-deformation during daily wear and washing.
[0003] At present, some functional fabrics commonly used on the market, such as modal fabrics, pure cotton fabrics, etc., have relatively simple functions. Although modal fabrics have good moisture absorption and breathability, they have low wear resistance and are more suitable for summer; although cotton fabrics have good moisture absorption and warmth retention, they are prone to shrinkage and deformation after long-term wearing, which reduces the comfort of using functional fabrics. Summary of the invention
[0004] In order to solve the problem that existing functional fabrics cannot simultaneously and well take into account moisture absorption and perspiration discharge, breathability and warmth retention, the present application provides a moisture absorption and perspiration-free breathable fabric and a preparation method thereof.
[0005] In a first aspect, the present application provides a breathable fabric that absorbs moisture and wicks perspiration, using the following technical solution: A breathable fabric with moisture absorption and perspiration removal is composed of a surface layer and an inner layer which are arranged in close contact. The surface layer is woven from a first blended yarn, which is made by blending the following fibers in percentage by weight: 52-56% acrylic fiber, 18-22% viscose fiber, 10-14% cupro-ammonia fiber and 12-16% spandex fiber; the inner layer is woven from a second blended yarn, which is made by blending the following fibers in percentage by weight: 58.5-62.5% acrylic fiber, 10-15% viscose fiber, 11.5-15.5% spandex fiber, 8-12% cupro-ammonia fiber and 3-4% wool.
[0006] By adopting the above technical scheme, acrylic fiber, viscose fiber, spandex fiber, cupro-ammonia fiber and wool in a relatively optimal dosage ratio are blended and woven to obtain an inner layer. Acrylic fiber has good warmth retention, elasticity and wear resistance, and viscose fiber has good moisture absorption and air permeability, softness and antistatic properties. The blending of the two can improve the moisture absorption and air permeability of the breathable fabric while also improving the warmth retention. However, the elasticity of the breathable fabric is insufficient and it is easy to deform after long-term wearing, which reduces the moisture absorption, air permeability and warmth retention of the breathable fabric. Therefore, on the basis of acrylic fiber and viscose fiber, spandex fiber, cupro-ammonia fiber and wool fiber are further added. The spandex fiber has good elasticity, It can further improve the elasticity of the breathable fabric and reduce the problem of deformation caused by long-term use; cuprammonia fiber is made from cotton seed fluff wrapped around cotton seeds, and the fluff part is refined and dissolved to prepare pure regenerated fiber. The fiber has uniform thickness and an approximately circular cross-section. It has good moisture absorption and air permeability, resilience, smoothness and soft skin-friendliness, and it will generate heat after absorbing moisture, which has a good warming effect; wool fiber has good skin-friendliness, moisture absorption and air permeability and warmth retention. The combination of the three can produce a good synergistic effect with viscose fiber and acrylic fiber. The breathable fabric made in this way has the properties of moisture absorption and air permeability, warmth retention, elasticity and non-deformation.
[0007] Acrylic fiber, viscose fiber, spandex fiber and cuprammonium fiber in an optimal dosage ratio are blended and woven to obtain a surface layer, which is fitted with an inner layer. The inner layer fabric fits the skin and needs to be soft, skin-friendly, warm, and breathable. The surface layer is away from the skin and in contact with the environment, and needs to have good moisture absorption and breathability, wear resistance and antistatic properties. By adjusting the different fiber blending proportions of the inner layer and the surface layer, a breathable fabric with good moisture absorption and breathability, warmth retention, elasticity and non-deformation properties can be obtained. It has the advantages of being warm in winter and cool in summer, has a wide range of applications, and can be widely used in underwear fabrics, such as thermal underwear, vests, suspenders, etc.
[0008] Preferably, the cuprammonia fiber is a pretreated cuprammonia fiber, and the pretreated cuprammonia fiber is prepared by pretreating the following raw materials in parts by weight: 1-3 parts of ammonium persulfate Disodium sulfosuccinate 1-2 parts 1.5-2.5 parts of ammonium lauryl sulfate Stabilizer 5-10 parts Dispersant 6-12 parts 80-120 parts of water.
[0009] By adopting the above technical scheme, disodium sulfosuccinate and ammonium dodecyl sulfate are used as surfactants, and ammonium persulfate is used as an activator. Ammonium persulfate has a good activation effect and can activate the surface of the cuprammonia fiber, thereby improving the surface wetting and penetration of disodium sulfosuccinate and ammonium dodecyl sulfate on the cuprammonia fiber, thereby improving the penetration and dispersion and relaxation effects of the stabilizer and dispersant on the cuprammonia fiber. The cuprammonia fiber prepared in this way has good dispersibility and fluffy fiber structure, can be evenly dispersed with other fibers during the blending process, improves the fluffiness of the prepared breathable fabric, and then improves the moisture absorption, air permeability and warmth retention of the prepared breathable fabric. At the same time, due to the fluffy fiber structure of the cuprammonia fiber, the prepared breathable fabric has good elasticity and is not easy to deform during long-term wearing.
[0010] Preferably, the stabilizer consists of propylene glycol alginate and polyvinyl alcohol in a weight ratio of 1:(0.5-1).
[0011] By adopting the above technical scheme, using propylene glycol alginate and polyvinyl alcohol in an optimal dosage ratio as stabilizers, they can evenly penetrate and adhere to the surface of the cuprammonia fiber to form a uniform attachment film, thereby improving the uniform penetration and dispersion of the softening dispersant on the surface of the cuprammonia fiber and improving the fluffy and relaxing efficiency of the cuprammonia fiber.
[0012] Preferably, the dispersant is composed of polyether-modified polydimethylsiloxane and polyethylene glycol diglycidyl ether in a weight ratio of 1:(1-2).
[0013] By adopting the above technical scheme, using polyether-modified dimethylsiloxane and polyethylene glycol diglycidyl ether in an optimal dosage ratio as dispersants, the fluffiness and relaxation of the fiber structure of the cuprammonia fiber can be improved, and the obtained pretreated cuprammonia fiber has good dispersibility, softness, elasticity and moisture absorption and air permeability. The fluffy fiber structure makes the obtained breathable fabric not easy to deform during long-term use, and can maintain good fabric dimensional stability.
[0014] Preferably, the pretreated cuprammonia fiber is prepared by the following steps: A1. Add ammonium persulfate, disodium sulfosuccinate and ammonium dodecyl sulfate into water, stir well, then add cuprammonia fiber, mix and stir for 20-30 minutes to obtain a cuprammonia fiber dispersion; A2. Add stabilizer and dispersant to the cuprammonia fiber dispersion, heat and mix, then filter, wash and dry to obtain pretreated cuprammonia fiber.
[0015] By adopting the above technical scheme, ammonium sulfate, disodium sulfosuccinate and ammonium dodecyl sulfate are first used to activate and surface-wet the cuprammonia fiber to improve the dispersion performance of the cuprammonia fiber, and then a stabilizer and a dispersant are added. Under heating conditions, the stabilizer and the dispersant play a good synergistic role and can fully relax and fluff the cuprammonia fiber. After filtering, washing and drying, the cuprammonia fiber with a fluffy fiber structure is prepared.
[0016] Preferably, during pretreatment, the weight ratio of the cuprammonium fiber to the pretreatment liquid is 1:(10-20).
[0017] By adopting the above technical solution and using an optimal amount of pretreatment liquid to soak the cuprammonia fiber, the cuprammonia fiber can be fully fluffy.
[0018] Preferably, the mixing temperature in step A2 is 42-48° C., and the mixing time is 10-20 min.
[0019] By adopting the above technical solution, the optimal mixing temperature and mixing time can make the cuprammonia fiber fully fluffy without damaging the cuprammonia fiber.
[0020] Preferably, the specification of the first blended yarn is 30-50D, and the specification of the second blended yarn is 20-30D.
[0021] By adopting the above technical scheme, the fineness of the first blended yarn of the surface layer is set to be greater than the fineness of the second blended yarn of the inner layer, so that the inner layer of the breathable fabric has good density, skin-friendliness, warmth retention and moisture absorption and air permeability, while the surface layer has good perspiration absorption and air permeability, which is conducive to the discharge of sweat, thereby improving the moisture absorption and air permeability of the breathable fabric while having good warmth retention, and is not easy to deform after long-term use.
[0022] Preferably, the weight of the moisture wicking breathable fabric is 280-320 g / m 2 .
[0023] By adopting the above technical solution, the breathable fabric with better grammage has moderate density and can better balance moisture absorption, breathability and warmth retention.
[0024] In a second aspect, the present application provides a method for preparing a moisture absorbing and perspiration wicking breathable fabric, using the following technical solution: A method for preparing a moisture-absorbing and perspiration-wicking breathable fabric comprises the following preparation steps: S1, blending acrylic fiber, viscose fiber, cupro fiber and spandex fiber to obtain a first blended yarn, and weaving the first blended yarn to obtain a surface layer; S2, blending acrylic fiber, viscose fiber, cupro-ammonia fiber, spandex fiber and wool to obtain a second blended yarn, and weaving the second blended yarn to obtain an inner layer; S3, the surface layer and the inner layer are laminated together to obtain a breathable fabric that absorbs moisture and wicks perspiration.
[0025] By adopting the above technical solution, the woven inner layer and the surface layer are bonded together to prepare a breathable fabric with good moisture absorption and perspiration discharge, heat preservation and non-deformation properties.
[0026] In summary, this application has the following beneficial effects: 1. The moisture wicking breathable fabric of the present application is composed of a surface layer and an inner layer, the surface layer is made by blending and weaving acrylic fiber, viscose fiber, spandex fiber and cupro-ammonia fiber, and the inner layer is made by blending and weaving acrylic fiber, viscose fiber, spandex fiber, cupro-ammonia fiber and wool; the inner layer fabric fits the skin and needs to be soft, skin-friendly, warm and moisture-absorbing and breathable, while the surface layer is away from the skin and in contact with the environment, and needs to have good moisture-absorbing and breathable properties, wear resistance and antistatic properties; by adjusting the different fiber blending proportions of the inner layer and the surface layer, a breathable fabric with good moisture-absorbing and breathable properties, warmth retention, elasticity and non-deformation properties is obtained, which has the advantages of being warm in winter and cool in summer, and has a wide range of applications, and can be widely used in fabrics for underwear, such as thermal underwear, vests, suspenders, etc.
[0027] 2. The cuprammonium fiber is pretreated by using ammonium persulfate, disodium sulfosuccinate, ammonium dodecyl sulfate, a stabilizer, a dispersant and water, wherein the stabilizer is preferably composed of propylene glycol alginate and polyvinyl alcohol, and the dispersant is preferably composed of polyether-modified polydimethylsiloxane and polyethylene glycol diglycidyl ether, so as to obtain the pretreated cuprammonium fiber, which has good dispersibility and fluffiness, can be evenly dispersed with other fibers during the blending process, thereby improving the fluffiness of the obtained breathable fabric, and then improving the moisture absorption, air permeability and warmth retention of the obtained breathable fabric; at the same time, due to the fluffy fiber structure of the cuprammonium fiber, the obtained breathable fabric has good elasticity and is not easy to deform during long-term wearing.
[0028] 3. The preparation method of the present application is to bond the woven inner layer and the surface layer together to prepare a breathable fabric with good moisture absorption and perspiration discharge, heat preservation and non-deformation properties. DETAILED DESCRIPTION
[0029] The present application is further described in detail below with reference to examples.
[0030] The following are the sources and specifications of some raw materials of this application. The raw materials used in the preparation examples and embodiments of this application can be obtained from the market, including but not limited to the raw materials of the following models and manufacturers. Raw materials with equivalent performance can be used: 1. Acrylic fiber: produced by Toyobo Co., Ltd., with a fineness of 0.5-1.5dtex and a length of 30-45mm; 2. Viscose fiber: produced by Lenzing, with a fineness of 0.8-1.7dtex and a length of 35-40mm; 3. Cuprammonium fiber: Bemberg, fineness 1-1.6dtex, length 35-40mm; 4. Spandex fiber: produced by Toyobo Co., Ltd., with a fineness of 1-1.5dtex and a length of 35-40mm; 5. Wool: Commercially available fine wool, diameter 30-50 μm, length 50-70 mm; 6. Disodium sulfosuccinate: MES, solid content 30%, pH value (1% aqueous solution): 5-7; 7. Dodecyl ammonium sulfate: K12A, CAS No. 2235-54-3; 8. Propylene glycol alginate: CAS No. 9005-37-2, content 99%; 9. Polyvinyl alcohol: PVA 17-99H; 10. Polyether modified polydimethylsiloxane: Green Union, JH-3667; 11. Polyethylene glycol diglycidyl ether: KMIKE, CAS No. 39443-66-8, epoxy value 0.52.
[0031] Preparation example of pretreated cuprammonium fiber Preparation Example 1 Preparation Example 1 discloses a pretreated cuprammonia fiber, which is prepared by the following steps: A1. Add 1 kg of ammonium persulfate, 1 kg of disodium sulfosuccinate and 2 kg of ammonium dodecyl sulfate to 80 kg of water, stir well, then add 5.05 kg of cuprammonium fiber, mix and stir for 20-30 minutes to obtain a cuprammonium fiber dispersion; A2. Add 5 kg of polyvinyl alcohol as a stabilizer and 12 kg of polyether-modified polydimethylsiloxane as a dispersant to the cuprammonia fiber dispersion, heat to 42°C and mix and stir for 10 minutes, then filter, wash with water 2-3 times, and dry at 70°C to obtain pretreated cuprammonia fiber.
[0032] Preparation Example 2-3 The difference between Preparation Example 2-3 and Preparation Example 1 is that the amount of raw materials used and the preparation conditions are different, see Table 1 below for details.
[0033] Table 1 Raw material dosage and preparation conditions of Preparation Examples 1-3 Preparation Example 4 The difference between Preparation Example 4 and Preparation Example 1 is that the stabilizer is different. The stabilizer in Preparation Example 4 is composed of propylene glycol alginate and polyvinyl alcohol, and the weight ratio of propylene glycol alginate to polyvinyl alcohol is 1:0.5. The rest is the same as Preparation Example 1.
[0034] Preparation Example 5 The difference between Preparation Example 5 and Preparation Example 1 is that the weight ratio of propylene glycol alginate to polyvinyl alcohol is 1:1, and the rest is the same as Preparation Example 1.
[0035] Preparation Example 6 The difference between Preparation Example 6 and Preparation Example 5 is that an equal amount of propylene glycol alginate is replaced by hydroxyethyl cellulose, and the rest is the same as Preparation Example 1.
[0036] Preparation Example 7 The difference between Preparation Example 7 and Preparation Example 5 is that the dispersant is different. The dispersant in Preparation Example 6 is composed of polyether-modified polydimethylsiloxane and polyethylene glycol diglycidyl ether, and the weight ratio of polyether-modified polydimethylsiloxane and polyethylene glycol diglycidyl ether is 1:1. The rest is the same as Preparation Example 5.
[0037] Preparation Example 8 The difference between Preparation Example 8 and Preparation Example 5 is that the weight ratio of polyether-modified polydimethylsiloxane to polyethylene glycol diglycidyl ether is 1:2, and the other parts are the same as Preparation Example 5.
[0038] Preparation Example 9 The difference between Preparation Example 9 and Preparation Example 8 is that an equal amount of polyethylene glycol diglycidyl ether is replaced by polyethylene glycol 400, and the rest is the same as Preparation Example 8.
[0039] Preparation Example 10 The difference between Preparation Example 10 and Preparation Example 1 is that an equal amount of ammonium dodecyl sulfate is replaced by disodium sulfosuccinate, and the rest is the same as Preparation Example 1.
[0040] Preparation Comparative Example 1 The difference between Preparation Comparative Example 1 and Preparation Example 1 is that the amount of stabilizer used is 2 kg, the amount of dispersant used is 15 kg, and the rest is the same as Preparation Example 1. Example
[0041] Example 1 Embodiment 1 discloses a breathable fabric with moisture absorption and perspiration removal, which is provided by laminating a surface layer and an inner layer, wherein the surface layer is woven from a first blended yarn, and the inner layer is woven from a second blended yarn, wherein the first blended yarn is blended from the following fibers in percentage by weight: 52% acrylic fiber, 22% viscose fiber, 10% cuprammonium fiber, and 16% spandex fiber; The second blended yarn is made by blending the following fibers in percentage by weight: 58.5% acrylic fiber, 15% viscose fiber, 15.5% spandex fiber, 8% cupro fiber and 3% wool.
[0042] The moisture wicking breathable fabric is made by the following steps: S1, blending acrylic fiber, viscose fiber, cupro fiber and spandex fiber according to the above amounts to obtain a first blended yarn, the specification of the first blended yarn is 30D, and weft knitting the first blended yarn to obtain a surface layer; S2, blending acrylic fiber, viscose fiber, cupro-ammonia fiber, spandex fiber and wool according to the above amounts to obtain a second blended yarn, the specification of the second blended yarn is 20D, and the second blended yarn is weft-knitted to obtain an inner layer; S3. Use polyurethane hot melt adhesive to bond the surface layer and the inner layer. The coating amount of polyurethane hot melt adhesive is 8g / m 2 The polyurethane hot melt adhesive is a commercially available polyurethane hot melt adhesive for fabric bonding, and the model is not limited. The moisture-absorbing and perspiration-wicking breathable fabric is prepared in this way. The weight of the moisture-absorbing and perspiration-wicking breathable fabric prepared in this embodiment is 280g / square meter.
[0043] Example 2-3 The difference between Example 2-3 and Example 1 is that the amounts of raw materials used are different, see Table 2 below for details.
[0044] Table 2 Preparation parameters of Examples 1-3 Embodiment 4-14 The difference between Example 4-14 and Example 2 is that the sources of the cuprammonia fiber are different, see Table 3 below for details.
[0045] Table 3 Sources of the cuprammonia fibers of Examples 4-14 Example Preparation Example Example 4 Preparation Example 1 Example 5 Preparation Example 2 Example 6 Preparation Example 3 Example 7 Preparation Example 4 Example 8 Preparation Example 5 Example 9 Preparation Example 6 Example 10 Preparation Example 7 Embodiment 11 Preparation Example 8 Example 12 Preparation Example 9 Example 13 Preparation Example 10 Embodiment 14 Preparation Comparative Example 1 Comparative Example Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that the cuprammonium fiber in the second blended yarn is replaced by viscose fiber in equal amount, and the rest is the same as Example 1.
[0046] Comparative Example 2 An equal amount of wool in the second blended yarn is replaced by modal fiber, which is from Lenzing and has a fineness of 1-1.5 dtex and a length of 35-40 mm; the rest is the same as in Example 1.
[0047] Performance Testing The following performance tests were conducted on the moisture wicking breathable fabrics prepared in Examples 1-14 and Comparative Examples 1-2: 1. Moisture absorption and perspiration test According to the test method in GB / T 21655.2-2019, test the water absorption rate A (unit: % / s), test and record the test results; 2. Air permeability test According to the test method in GB / T 5453-1997, test the air permeability (unit: mm / s), test and record the test results; 3. Thermal insulation test: Test according to method A in GB / T 11048-1989, test the thermal insulation rate (unit: %), test and record the test results; 4. Resilience test: According to the test method in FZ / T 70006-2022, test the elastic recovery rate (unit: %) after one stretch under a fixed force, and test and record the test results.
[0048] The following are the performance test data of the moisture wicking breathable fabrics prepared in Examples 1-14 and Comparative Examples 1-2, see Table 4 below for details.
[0049] Table 4 Performance test data of Examples 1-14 and Comparative Examples 1-2 Combining Examples 1-3 and Comparative Examples 1-2 and Table 4, it can be seen that the breathable fabric prepared by using acrylic fiber, viscose fiber, cuprammonium fiber, spandex fiber and wool blended weaving in a better dosage ratio as the inner layer fabric has good moisture absorption and air permeability, thermal insulation and resilience. In Comparative Example 1, cuprammonium fiber is replaced with viscose fiber, and in Comparative Example 2, wool is replaced with modal fiber, and the moisture absorption and air permeability, thermal insulation and resilience of the breathable fabric prepared are all reduced.
[0050] It can be seen from Examples 1-3 and Examples 4-14 and Table 4 that the use of the pretreated cuprammonia fiber of the present application can further improve the moisture absorption and air permeability, thermal insulation and resilience of the prepared breathable fabric.
[0051] Compared with Examples 4-6, Examples 7-8 use propylene glycol alginate and polyvinyl alcohol in a better dosage ratio as stabilizers, and in Example 9, propylene glycol alginate is replaced with hydroxyethyl cellulose. From the data, it can be seen that the performance of the breathable fabric in Examples 7-8 is significantly better than that of the breathable fabric in Examples 4-6 and 9, indicating that propylene glycol alginate and polyvinyl alcohol in a better dosage ratio have a good synergistic effect, which can better improve the adhesion and permeability to cuprammonia fibers, thereby improving the moisture absorption and air permeability, thermal insulation and resilience of the breathable fabric obtained.
[0052] Compared with Examples 7-8, Examples 10-11 further use polyether-modified polydimethylsiloxane and polyethylene glycol diglycidyl ether in a preferred dosage ratio as dispersants, and in Example 12, polyethylene glycol 400 is used to replace polyethylene glycol diglycidyl ether. In Example 14, the stabilizer is reduced and the dispersant is increased. From the above data, it can be seen that the performance of the breathable fabric in Examples 10-11 is significantly better than that of the breathable fabric in Examples 7-8, Example 12 and Example 14, indicating that the polyether-modified polydimethylsiloxane and polyethylene glycol diglycidyl ether in a preferred dosage ratio have a good synergistic effect, and can cooperate with the stabilizer to thereby improve the moisture absorption and air permeability, thermal insulation and resilience of the obtained breathable fabric.
[0053] In Example 13, compared with Example 4, the performance of the breathable fabric obtained by replacing ammonium dodecyl sulfate with disodium sulfosuccinate is reduced, which may be because the wetting effect on the surface of the cuprammonium fiber is reduced, thereby reducing the stretching and fluffing efficiency of the dispersant and stabilizer on the cuprammonium fiber.
[0054] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A breathable fabric that absorbs moisture and wicks away perspiration, characterized in that: The invention is composed of a surface layer and an inner layer which are laminated together, wherein the surface layer is woven from a first blended yarn, wherein the first blended yarn is made by blending fibers in the following weight percentages: 52-56% acrylic fiber, 18-22% viscose fiber, 10-14% cupro-ammonia fiber and 12-16% spandex fiber; and the inner layer is woven from a second blended yarn, wherein the second blended yarn is made by blending fibers in the following weight percentages: 58.5-62.5% acrylic fiber, 10-15% viscose fiber, 11.5-15.5% spandex fiber, 8-12% cupro-ammonia fiber and 3-4% wool.
2. A moisture wicking breathable fabric according to claim 1, characterized in that: The copper-ammonia fiber is a pretreated copper-ammonia fiber, and the pretreated copper-ammonia fiber is prepared by pretreating the following raw materials in parts by weight: 1-3 parts of ammonium persulfate Disodium sulfosuccinate 1-2 parts 1.5-2.5 parts of ammonium lauryl sulfate Stabilizer 5-10 parts Dispersant 6-12 parts 80-120 parts of water.
3. A moisture wicking breathable fabric according to claim 2, characterized in that: The stabilizer consists of propylene glycol alginate and polyvinyl alcohol in a weight ratio of 1:(0.5-1).
4. A moisture wicking breathable fabric according to claim 2, characterized in that: The dispersant is composed of polyether-modified polydimethylsiloxane and polyethylene glycol diglycidyl ether in a weight ratio of 1:(1-2).
5. A moisture wicking breathable fabric according to any one of claims 2 to 4, characterized in that the pretreated cuprammonia fiber is prepared by the following steps: A1. Add ammonium persulfate, disodium sulfosuccinate and ammonium dodecyl sulfate into water, stir well, then add cuprammonia fiber, mix and stir for 20-30 minutes to obtain a cuprammonia fiber dispersion; A2. Add stabilizer and dispersant to the cuprammonia fiber dispersion, heat and mix, then filter, wash and dry to obtain pretreated cuprammonia fiber.
6. A moisture wicking breathable fabric according to claim 5, characterized in that: During pretreatment, the weight ratio of the cuprammonium fiber to the pretreatment liquid is 1:(10-20).
7. The moisture wicking breathable fabric according to claim 5, characterized in that: The mixing temperature in step A2 is 42-48° C., and the mixing time is 10-20 min.
8. The moisture wicking breathable fabric according to claim 1, characterized in that: The specification of the first blended yarn is 30-50D, and the specification of the second blended yarn is 20-30D.
9. The moisture wicking breathable fabric according to claim 1, characterized in that: The weight of the moisture wicking breathable fabric is 280-320g / m 2 .
10. A method for preparing a moisture wicking breathable fabric according to any one of claims 1 to 9, characterized in that: The method comprises the following preparation steps: S1, blending acrylic fiber, viscose fiber, cupro fiber and spandex fiber to obtain a first blended yarn, and weaving the first blended yarn to obtain a surface layer; S2, blending acrylic fiber, viscose fiber, cupro-ammonia fiber, spandex fiber and wool to obtain a second blended yarn, and weaving the second blended yarn to obtain an inner layer; S3, the surface layer and the inner layer are laminated together to obtain a breathable fabric that absorbs moisture and wicks perspiration.
Citation Information
Patent Citations
Antibacterial heat-preserving underwear fabric and preparation method thereof
CN104382245A
Soft and moist skin-friendly fabric containing protein components as well as preparation process and application of soft and moist skin-friendly fabric
CN117845418A
Self-heating silk double-sided fabric weaving structure