Leather-imitated water-based synthetic leather and preparation method thereof
By using the intermediate layer without adding crosslinking agent and the post-kneading treatment liquid during the preparation of the aqueous synthetic leather, combined with the aqueous polyurethane resin with high and low Young's modulus, a different shrinkage effect of the surface layer, the intermediate layer and the bottom layer are formed. The existing water-based synthetic leather pattern is solved and the lack of leather feel is insufficient, and a more three-dimensional and strong leather feel is achieved.
Patent Information
- Application Number
- CN202411151408.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-12-03
AI Technical Summary
The existing water-based synthetic leather cannot shrink after cross-linking and shaping of the foam layer, and has poor elasticity, resulting in dull, non-three-dimensional patterns, and insufficient leather feel.
The kneading treatment liquid is prepared by crosslinking agent. The intermediate layer without adding crosslinking agent during the preparation process ensures shrinkable and deformable characteristics, and kneading in the later stage to form different shrinkage effects of the surface layer, intermediate layer and bottom layer, combined with Water-based polyurethane resin with high Young's modulus and fillers with low Young's modulus form dermis-like patterns.
It improves the three-dimensionality and leather feel of synthetic leather, provides a richer style and strong leather effect, enhances elasticity, and avoids the defect of poor pressing creases.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water-based leather, and in particular relates to a simulated leather water-based synthetic leather and a preparation method thereof. Background Art
[0002] With the progress of society, people's environmental awareness is gradually enhanced. With the progress of society, people's environmental awareness is gradually enhanced. Water-based synthetic leather prepared with water-based polyurethane as raw material is gradually replacing solvent-based synthetic leather prepared with solvent-based PU using DMF, toluene and xylene as solvents.
[0003] At present, the preparation method of water-based synthetic leather is to use thermosetting polyether water-based polyurethane resin to make a 15×10 unit block with a single texture on release paper or embossing, and then splice several unit blocks into a whole, and add a cross-linking agent to the foaming layer. After the foaming layer is cross-linked and fixed, the prepared synthetic leather cannot shrink and has poor resilience, making the prepared texture dull and not three-dimensional. Alternatively, a kneading process is performed after the foaming layer is cross-linked and fixed, making the material of the synthetic leather softer, but the leather feel of the final synthetic leather is still insufficient.
[0004] Therefore, there is an urgent need for a simulated leather water-based synthetic leather and a preparation method thereof to solve the above problems. Summary of the invention
[0005] In order to overcome the defects in the prior art, the present invention provides a simulated leather water-based synthetic leather and a preparation method thereof. The water-based synthetic leather prepared by the present invention has better three-dimensional sense and genuine leather feel.
[0006] To achieve one of the above purposes, the present invention adopts the following technical solution:
[0007] A method for preparing simulated leather water-based synthetic leather, the specific steps are as follows:
[0008] S1. Slurry preparation: Select raw materials containing water-based polyurethane resin to prepare surface slurry, middle layer slurry and bottom layer slurry respectively, and use cross-linking agent to prepare rubbing treatment liquid; the surface layer slurry is made of polyester thermoplastic water-based polyurethane resin, and no cross-linking agent is added to the middle layer slurry to ensure the shrinkable and deformable characteristics of the foaming layer;
[0009] S2, coating the surface layer slurry on the release paper and drying to obtain the surface layer, coating the middle layer slurry on the surface layer and drying to obtain the middle layer, coating the bottom layer slurry on the middle layer to obtain the bottom layer, laminating the bottom layer with the base fabric, and then drying, shaping, and peeling in sequence to obtain the semi-finished product;
[0010] S3, performing surface modification treatment on the surface layer of the semi-finished product, then immersing the semi-finished product in the prepared rubbing treatment liquid, and finally putting it into a rubbing machine for rubbing to make water-based synthetic leather.
[0011] Preferably, the Young's modulus of the surface layer is 3-5 MPa, and the Young's modulus of the middle layer and the Young's modulus of the bottom layer are both 0.8-1.2 MPa.
[0012] Preferably, the wrinkle treatment liquid is one of aziridine with a mass concentration of 0.2-2.0% or carbodiimide dilution with a mass concentration of 0.2-2.0%.
[0013] Preferably, the surface slurry is prepared from waterborne polyurethane resin, defoamer, wetting and leveling agent and thickener in a mass ratio of 100:(0.2-0.5):(0.5-2.0):(0.2-1.0);
[0014] Preferably, the middle layer and the bottom layer are prepared from waterborne polyurethane resin, filler and foaming agent in a mass ratio of 100:(20-40):(4-6) (the filler can reduce the elasticity of the resin itself and improve the shrinkage of the middle layer and the bottom layer).
[0015] Preferably, both the middle layer and the bottom layer are formed into pores by mechanical foaming, and the foaming ratio is ≥ 2.5 times, which is beneficial to the stability of the foam.
[0016] Preferably, the filler is one of kaolin and pyrophyllite powder.
[0017] To achieve the second purpose above, the present invention provides a water-based synthetic leather prepared by a method for preparing a simulated leather water-based synthetic leather, wherein the water-based synthetic leather comprises a surface layer, an intermediate layer, a bottom layer and a base fabric connected in sequence.
[0018] The advantages of the present invention are:
[0019] (1) The present invention ensures the shrinkage and deformation characteristics of the middle layer by not adding a cross-linking agent in the early stage of preparing the middle layer, and adds a rubbing treatment liquid in the later stage, so that the synthetic leather is reshaped after shrinking, and after being rubbed by external force, the surface layer, the middle layer and the bottom layer have different shrinkage effects, making the synthetic leather more three-dimensional, and obtaining a texture similar to that of genuine leather, providing a richer style and a stronger genuine leather effect.
[0020] (2) The method of the present invention adopts a water-based polyurethane with a high Young's modulus as the surface layer, and adopts a water-based polyurethane with a low Young's modulus and a filler with poor elasticity for high foaming of the middle layer and the bottom layer. The surface layer has a high Young's modulus and low elasticity, and forms a large difference in shrinkage ratio between the middle layer and the bottom layer. After being rubbed with external force, the surface layer has different shrinkage effects from the middle layer and the bottom layer, forming a texture similar to that of genuine leather, thereby producing a shrinkable water-based leather.
[0021] (3) The intermediate layer prepared by the present invention does not add a cross-linking agent, thereby ensuring the shrinkable and deformable characteristics of the intermediate layer, and a certain concentration of a cross-linking agent is prepared as a grain treatment liquid, and the shrinkage of the intermediate layer is fixed by adding a post-treatment cross-linking agent, so that the resilience of the shrinkable water-based leather is improved after the grain is formed, thereby avoiding the defect of poor crease marks.
[0022] (4) The synthetic leather in the present invention is divided into a surface layer, an intermediate layer and a bottom layer; the surface layer is a coating layer, the intermediate layer is a foaming layer, which mainly provides hand feel and texture support, and the bottom layer is an adhesive layer, which serves to bond the intermediate layer to the base fabric. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.
[0024] The utility model discloses an imitation leather water-based synthetic leather, which consists of a surface layer, an intermediate layer, a bottom layer and a base fabric which are connected in sequence.
[0025] Example 1
[0026] A method for preparing artificial leather water-based synthetic leather specifically comprises the following steps:
[0027] (1) Preparation of surface slurry
[0028] Waterborne polyurethane resin model KT707H: 100 parts by mass;
[0029] Defoaming agent: 0.3 parts by mass;
[0030] Wetting and leveling agent: 1.0 parts by mass;
[0031] Thickener: 0.5 parts by mass.
[0032] (2) Preparation of middle layer slurry and bottom layer slurry
[0033] Waterborne polyurethane resin of model KT750D: 100 parts by mass;
[0034] Kaolin: 20 parts by mass;
[0035] Foaming agent: 5 parts by mass, the middle layer is foamed 2.8 times.
[0036] (3) Preparation of wrinkle treatment solution
[0037] Aziridine: 0.3 parts by mass;
[0038] Water: 99.7 parts by mass;
[0039] (4) coating the surface layer slurry on the release paper, coating the middle layer slurry on the surface layer after drying, coating the bottom layer slurry on the middle layer after drying, laminating the base fabric and the bottom layer through a laminating device, drying, shaping, and peeling to obtain a semi-finished product;
[0040] (5) After the semi-finished product has been subjected to a surface modification treatment step, it is immersed in a graining treatment liquid and then placed in a graining machine for kneading to obtain a finished water-based synthetic leather product 1.
[0041] The shrinkage rate of the water-based synthetic leather 1 was tested, and the radial shrinkage rate was measured to be 10.5%, and the weft shrinkage rate was 8.2%.
[0042] Example 2
[0043] A method for preparing artificial leather water-based synthetic leather specifically comprises the following steps:
[0044] (1) Preparation of surface slurry
[0045] WR111 waterborne polyurethane resin: 100 parts by mass;
[0046] Defoaming agent: 0.2 parts by mass;
[0047] Wetting and leveling agent: 1.5 parts by mass;
[0048] Thickener: 0.6 parts by mass;
[0049] (2) Preparation of middle layer slurry and bottom layer slurry
[0050] Waterborne polyurethane resin model KT751G: 100 parts by mass;
[0051] Kaolin: 30 parts by mass;
[0052] Foaming agent: 5 parts by mass, the middle layer is foamed 3.3 times.
[0053] (3) Preparation of wrinkle treatment solution
[0054] Carbodiimide: 2.0 parts by mass;
[0055] Water: 98 parts by mass.
[0056] (4) coating the surface layer slurry on the release paper, coating the middle layer slurry on the surface layer after drying, coating the bottom layer slurry on the middle layer after drying, laminating the base fabric with a laminating device, and obtaining a semi-finished product after drying and shaping;
[0057] (5) After the semi-finished product has been subjected to a surface modification treatment step, it is immersed in a graining treatment liquid and then placed in a graining machine for kneading to obtain a water-based synthetic leather product 2.
[0058] The shrinkage rate of the water-based synthetic leather 2 was tested, and the radial shrinkage rate was 9.6%, and the weft shrinkage rate was 7.9%.
[0059] According to the shrinkage test of Examples 1-2, the water-based synthetic leather finished product 1 and the water-based synthetic leather finished product 2 prepared in Examples 1-2 have more three-dimensional textures and varied styles, which are closer to the textures of genuine leather.
[0060] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a simulated leather water-based synthetic leather, characterized in that: The specific steps are as follows: S1. Slurry preparation: selecting raw materials including waterborne polyurethane resin to prepare surface slurry, middle layer slurry and bottom layer slurry respectively, and using a cross-linking agent to prepare a rubbing treatment liquid; the surface layer slurry is made of polyester thermoplastic waterborne polyurethane resin, and no cross-linking agent is added to the middle layer slurry; S2, coating the surface layer slurry on the release paper and drying to obtain the surface layer, coating the middle layer slurry on the surface layer and drying to obtain the middle layer, coating the bottom layer slurry on the middle layer to obtain the bottom layer, laminating the bottom layer with the base fabric, and then drying, shaping, and peeling in sequence to obtain the semi-finished product; S3, performing surface modification treatment on the surface layer of the semi-finished product, then immersing the semi-finished product in the prepared rubbing treatment liquid, and finally putting it into a rubbing machine for rubbing to make water-based synthetic leather.
2. The method for preparing the artificial leather water-based synthetic leather according to claim 1, characterized in that: The Young's modulus of the surface layer is 3-5 MPa, and the Young's modulus of the middle layer and the Young's modulus of the bottom layer are both 0.8-1.2 MPa.
3. The method for preparing the artificial leather water-based synthetic leather according to claim 1, characterized in that: The wrinkle treatment liquid is one of aziridine with a mass concentration of 0.2-2.0% or carbodiimide dilution with a mass concentration of 0.2-2.0%.
4. The method for preparing the artificial leather water-based synthetic leather according to claim 1, characterized in that: The surface layer slurry is prepared from waterborne polyurethane resin, defoamer, wetting and leveling agent and thickener in a mass ratio of 100:(0.2-0.5):(0.5-2.0):(0.2-1.0).
5. The method for preparing the artificial leather water-based synthetic leather according to claim 1, characterized in that: The middle layer and the bottom layer are both prepared from waterborne polyurethane resin, filler and foaming agent in a mass ratio of 100:(20-40):(4-6).
6. The method for preparing the artificial leather water-based synthetic leather according to claim 1, characterized in that: The middle layer and the bottom layer are both formed of foam cells by mechanical foaming, and the foaming ratio is ≥2.5 times.
7. The method for preparing the artificial leather water-based synthetic leather according to claim 5, characterized in that: The filler is one of kaolin and pyrophyllite powder.
8. A water-based synthetic leather obtained by the method for preparing a simulated leather water-based synthetic leather according to any one of claims 1 to 7, characterized in that: The water-based synthetic leather consists of a surface layer, an intermediate layer, a bottom layer and a base fabric which are connected in sequence.