Multi-layer fireproof protection system and construction method thereof

By adopting a composite fire protection system in high-rise/super-high-rise buildings, combining the interface layer, fire insulation layer and decorative fire resistance layer, the problem of poor fire resistance in steel structures is solved, and cost-effective fire resistance is achieved, which can effectively withstand high temperatures. Roast and extend fire resistance.

CN119062018APending Publication Date: 2024-12-03SICHUAN FIRE RES INST OF MEM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411023996.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The steel structure has poor fire resistance in high-rise/super-high-rise buildings. The traditional single-structure fire protection system is difficult to take into account both fire resistance and heat insulation, and cannot effectively improve the fire safety of the building.

Method used

Adopt a multi-layer fire protection system, including an interface layer, a fire insulation layer and a decorative fire-resistant layer. Through the combination of interface agent and fire insulation coating, a multi-layer structure is formed to prevent heat transfer and resist high temperature scorching, and improve the fire-resistant coating. integrity.

Benefits of technology

It achieves the same-stop improvement of fire resistance and heat insulation, can withstand high temperatures above 1100℃, extend the fire resistance time of the steel structure, and improve the fire safety of the building.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119062018A_ABST
    Figure CN119062018A_ABST
Patent Text Reader

Abstract

The invention discloses a multi-layer fireproof protection system and a construction method thereof, and relates to the technical field of fireproof protection systems. The multi-layer fireproof protection system comprises an interface layer, a fireproof heat insulation layer and a facing fireproof layer. Wherein the interface layer is formed by uniformly coating an interface agent on the surface of a steel structure; the fireproof heat-insulating coating layer is formed by smearing fireproof heat-insulating coating on the surface of the interface layer; and the facing fire-resistant layer is a facing coiled material coated with facing fire-resistant powder. The invention further discloses a construction method of the multi-layer fireproof protection system. The multi-layer fireproof protection system has fire resistance, aging resistance and decoration effects at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fire protection systems, and in particular to a multi-layer fire protection system and a construction method thereof. Background Art

[0002] When a fire accident occurs in a high-rise / super high-rise building, the vertical spread speed is fast, there are many combustibles, external rescue is difficult, the risk of smoke and toxic gases is high, and the main rescue means are scarce. High-rise / super high-rise buildings still mainly rely on self-rescue. Therefore, improving the fire resistance limit of high-rise / super high-rise buildings is the primary issue to improve the fire safety of high-rise / super high-rise buildings.

[0003] The general structure of high-rise buildings is reinforced concrete structure, steel structure, steel-concrete composite structure, etc. In particular, super high-rise structures are mostly in the form of steel-concrete structure or pure steel structure. This structure has high strength and rigidity, can withstand large loads, and has good ductility and plastic deformation capacity. The fire resistance of concrete structure is relatively good. Concrete is a non-combustible material with good fire resistance. Its fire resistance is mainly due to the concrete aggregate inside it, which is usually a hard, dense mineral material with high fire resistance. Therefore, the fire resistance of concrete structure is relatively strong. The fire resistance of steel structure is relatively poor. At high temperatures, the strength and elastic modulus of steel will drop significantly, and may even cause structural damage. Therefore, for steel structure buildings, fire prevention measures are usually required, such as applying fire retardant coatings, setting up fire partitions, etc., to improve their fire resistance.

[0004] According to the fire protection characteristics of high-rise / super-high-rise buildings, it is urgent to develop a fire protection system that meets the characteristics of high-rise / super-high-rise buildings in order to meet the requirements of fire protection materials such as high fire resistance limit, good weather resistance, good flexibility, high strength, easy construction, and low surface density. The traditional fire protection system is a single-structure fire protection coating. This single-structure fire protection system is difficult to take into account both fire resistance and thermal insulation. In order to improve the above situation, the fire protection system should develop in the direction of multiple layers or multiple layers, and match fire protection coatings with different characteristics according to the temperature when exposed to fire, so as to achieve cost-effective fire protection performance. Summary of the invention

[0005] The purpose of the present invention is to provide a multi-layer fire protection system and a construction method thereof, which take into account both fire resistance and heat insulation. The multi-layer fire protection system of the present invention comprises an interface layer, a fireproof and heat-insulating layer and a facing fire-resistant layer. The interface layer is a bonding layer between the steel structure and the fireproof and heat-insulating layer; the fireproof and heat-insulating layer mainly plays a heat-insulating role to prevent the transfer of heat; the facing fire-resistant layer mainly ensures the integrity of the fireproof coating and can withstand baking above 1100°C to ensure the integrity of the fireproof coating.

[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0007] A multilayer fire protection system comprises an interface layer, a fireproof and heat-insulating layer and a finishing fire-resistant layer; wherein the interface layer is formed by evenly coating an interface agent on the surface of a steel structure; the fireproof and heat-insulating coating layer is formed by smearing a fireproof and heat-insulating coating on the surface of the interface layer; the finishing fire-resistant layer is a finishing coil coated with finishing fire-resistant layer powder, which is bonded to the fireproof and heat-insulating coating layer via an interface agent.

[0008] Furthermore, the interface agent is made of the following raw materials in parts by weight: 30-40 parts of flame retardant emulsion 907, 25-40 parts of solid mixture, 1-3 parts of alcohol ester dodecahydrate, 15-30 parts of glass microspheres, 0.08-0.15 parts of hydroxypropyl cellulose ether, and 10-40 parts of water;

[0009] Preferably, the interface agent is made of the following raw materials in parts by weight: 90740 parts of flame retardant emulsion, 35 parts of solid mixture, 2 parts of alcohol ester, 22 parts of glass microspheres, 0.1 parts of hydroxypropyl cellulose ether, and 20-30 parts of water.

[0010] Furthermore, the solid mixture includes silicon micropowder, alumina, and bentonite in a mass ratio of 6-10: 0.3-1.5: 0.05-0.15;

[0011] Preferably, the solid mixture includes silicon micropowder, alumina and bentonite in a mass ratio of 8:1:0.1.

[0012] Furthermore, the preparation method of the interface agent is as follows:

[0013] S11, weighing the raw materials in parts by weight;

[0014] S12, adding water into a blender, and pouring in a portion of alcohol ester 12, preferably, the mass of the portion of alcohol ester 12 is 1 / 2 of the total weight of alcohol ester 12;

[0015] S13, start the stirrer, slowly add hydroxypropyl cellulose ether and stir, preferably, the stirring speed is 1200-1800 r / min, and the stirring time is 15-30 min;

[0016] S14, reducing the stirring speed, slowly adding the solid mixture for stirring, preferably, the stirring speed is 800-1000 r / min, and the stirring time is 15-25 min;

[0017] S15. Add flame retardant emulsion 907 while stirring;

[0018] S16, pour in the remaining alcohol ester 12;

[0019] S17, reducing the stirring speed, slowly adding the vitrified microbeads and stirring to obtain the interface agent. Preferably, the stirring speed is 450-600 r / min, and the stirring time is 15-25 min.

[0020] Further, the fireproof and heat-insulating coating comprises the following raw materials in parts by weight: 800-1200 parts of black silicate binder, 150-220 parts of white silicate binder, 120-180 parts of expanded perlite, 650-1000 parts of expanded vermiculite, 10-30 parts of floating beads, 150-300 parts of mica, 1.0-5 parts of hydroxypropyl cellulose ether, 0.15-0.3 parts of sodium α-olefin sulfonate, 2-5 parts of zirconium-containing aluminum silicate fiber, and 35-60 parts of alumina fiber;

[0021] Preferably, the fireproof and heat-insulating coating is made of the following raw materials in parts by weight: 900 parts of black silicate binder, 180 parts of white silicate binder, 150 parts of expanded perlite, 850 parts of expanded vermiculite, 20 parts of floating beads, 220 parts of mica, 3 parts of hydroxypropyl cellulose, 0.2 parts of sodium α-olefin sulfonate, 4 parts of zirconium-containing aluminum silicate fiber, and 50 parts of alumina fiber.

[0022] The binder in the fire-retardant and heat-insulating coating can improve the strength of the fire-retardant and heat-insulating layer; mica can improve the ablation resistance of the fire-retardant and heat-insulating layer; alumina fiber can improve the cracking resistance of the fire-retardant and heat-insulating layer; relying solely on a single white silicate binder or a black silicate binder is not conducive to maintaining the volume stability of the fire-retardant coating at high temperatures. Therefore, a composite system of white silicate and black silicate binders is used to improve the stability of the fire-retardant and heat-insulating layer.

[0023] Furthermore, the preparation method of the fireproof and heat-insulating coating is as follows:

[0024] S21, weighing the raw materials in parts by weight;

[0025] S22, start the mixer, add zirconium-containing aluminum silicate fiber and aluminum oxide fiber in sequence and stir, preferably, the stirring time is 5 to 10 minutes;

[0026] S23, add expanded perlite, expanded vermiculite, floating beads, mica, hydroxypropyl cellulose, and sodium α-olefin sulfonate in sequence and continue stirring. Preferably, the stirring time is 3 to 5 minutes;

[0027] S24. Finally, add the black silicate binder and the white silicate binder and continue stirring to obtain the fireproof and heat-insulating coating. Preferably, the stirring time is 5 to 10 minutes.

[0028] Further, the facing refractory layer powder includes the following raw materials in parts by weight: 15-30 parts of diatomaceous earth, 8-15 parts of closed-cell perlite, 60-100 parts of expanded vermiculite, 15-25 parts of microspheres, 150-280 parts of alumina fiber, 300-700 parts of aluminum silicate fiber, 8-15 parts of silicon carbide powder, 2-6 parts of zirconium-containing aluminum silicate fiber, 2-8 parts of polyvinyl alcohol powder, 18-40 parts of latex powder, and 0.1-0.3 parts of ultramarine;

[0029] Preferably, the facing refractory layer powder is made of the following raw materials in parts by weight: 20 parts of diatomaceous earth, 12 parts of closed-cell perlite, 80 parts of expanded vermiculite, 20 parts of microspheres, 200 parts of alumina fiber, 500 parts of aluminum silicate fiber, 10 parts of silicon carbide powder, 4 parts of zirconium-containing aluminum silicate fiber, 3 parts of polyvinyl alcohol powder, 30 parts of latex powder, and 0.2 parts of ultramarine.

[0030] Furthermore, the particle size of the closed-cell perlite is 8 to 120 meshes, preferably 20 meshes;

[0031] Or / and the particle size of expanded vermiculite is 15 to 100 meshes, preferably 40 meshes;

[0032] The particle size of the microbeads is 10 to 180 mesh, preferably 50 mesh.

[0033] The facing fireproof layer is located at the outermost layer of the multi-layer fire protection system, directly facing the impact of high-temperature flames. The present invention prefers fibers with high fire resistance: alumina fibers, alumina fibers, zirconium-containing aluminum silicate fibers,

[0034] Furthermore, the preparation method of the facing refractory layer is as follows:

[0035] S31, weighing the raw materials in parts by weight;

[0036] S32, start the mixer, add the raw materials in sequence and stir to obtain a facing refractory layer powder, preferably, the stirring time is 20 to 40 minutes;

[0037] S33, evenly spreading the facing refractory layer powder on the facing coiled material cloth;

[0038] S34, prepare a binder solution, spray the binder solution on the flat facing refractory layer powder, and obtain the facing refractory layer after drying; preferably, the thickness of the facing refractory layer is 0.2-2 mm; preferably, the binder solution is a water glass solution, more preferably a water glass solution with a mass concentration of 5-20%, and further preferably a 10% water glass solution.

[0039] The present invention also provides a construction method of a multi-layer fire protection system, comprising the following steps:

[0040] S1. Remove debris from the surface of the steel structure, including rust, oil stains, and dust;

[0041] S2. Apply a layer of anti-rust primer on the surface of the steel structure and maintain it; preferably, the anti-rust primer is an epoxy zinc-rich anti-rust primer, and the coating thickness of the anti-rust primer is 40 to 80 μm; preferably, the anti-rust primer is maintained indoors; further preferably, the anti-rust primer is maintained indoors for 8 to 60 hours, more preferably for 24 hours;

[0042] S3. Uniformly apply the interface agent to the surface of the steel structure to form an interface layer; preferably, the coating thickness of the interface layer is 0.2 to 0.5 mm;

[0043] S4. When the interface layer is not completely dry, prepare the coating according to the mass ratio of fireproof and heat-insulating coating to water of 100:(180-250), spray or apply the coating on the surface of the interface layer to form a fireproof and heat-insulating coating layer; preferably, the first spraying is 3-5 mm, and each subsequent spraying or applying is 5-10 mm, until the thickness reaches 36-39 mm;

[0044] S5. According to the area of ​​the steel structure, cut the facing coil of the facing fire-resistant layer, evenly apply the interface agent on the bottom surface of the facing fire-resistant layer or the surface of the fire-proof and heat-insulating coating layer, stick the facing fire-resistant layer to the surface of the fire-proof and heat-insulating coating layer and then gently press to fix; preferably, the thickness of the facing fire-resistant layer is 0.2 to 2 mm.

[0045] S6. Curing the steel structure completed in S5; preferably, curing for 25 to 30 days.

[0046] Compared with the prior art, the present invention has the following beneficial effects:

[0047] The multi-layer fire protection system of the present invention includes an interface layer, a fireproof and heat-insulating layer, and a facing fire-resistant layer. The interface layer is the bonding layer between the steel structure and the fireproof and heat-insulating layer; the fireproof and heat-insulating layer mainly plays a heat-insulating role to prevent the transfer of heat; the facing fire-resistant layer mainly ensures the integrity of the fireproof coating and can withstand baking at temperatures above 1100°C to ensure the integrity of the fireproof coating. The present invention takes into account both fire resistance and heat insulation. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 This is a physical picture of the multi-layer fire protection system.

[0049] Figure 2 This is the overall result diagram of the outdoor exposure dripping natural aging test of Test Example 2.

[0050] Figure 3 This is a partial result diagram of the outdoor exposure dripping natural aging test of Test Example 2. DETAILED DESCRIPTION

[0051] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0052] Example 1

[0053] This embodiment discloses the multi-layer fire protection system and the construction method thereof of the present invention, which are specifically as follows:

[0054] 1. Interface agent:

[0055] Table 1-1 Ingredients of the interface agent of Example 1

[0056]

[0057]

[0058] The preparation method of the interface agent is as follows:

[0059] S11, weigh the raw materials in Table 1-1 according to the proportion;

[0060] S12, adding water into a blender, and pouring in 0.5 parts of alcohol ester twelve;

[0061] S13, start the mixer, set the mixer speed to 1500 r / min, slowly add hydroxypropyl cellulose ether, and stir for 20 min;

[0062] S14, adjust the mixer speed to 900r / min, and slowly add the solid mixed material into the mixing tank;

[0063] S15, pour in the flame retardant emulsion 907 while stirring;

[0064] S16, pour in the remaining alcohol ester 12;

[0065] S17. Reduce the speed of the mixer to 500 r / min, slowly add the vitrified microspheres, and continue stirring for 20 minutes to obtain a uniform and thick interface agent.

[0066] 2. Fireproof and heat-insulating coatings:

[0067] Table 1-2 Ingredients of fireproof and heat-insulating coating of Example 1

[0068] Serial number Raw material name Weight 1 Black silicate binder 900 2 White silicate binder 180 3 Expanded Perlite 150 4 Expanded Vermiculite 850 5 Floating beads 20 6 Mica 220 7 Hydroxypropyl Cellulose 3 8 Sodium α-olefin sulfonate 0.2 9 Zirconium-containing aluminum silicate fiber 4 10 Alumina Fiber 50

[0069] The preparation method of the fireproof and heat-insulating coating is as follows:

[0070] S21, weigh the raw materials in Table 1-2 according to the proportion;

[0071] S22, start the mixer, add zirconium-containing aluminum silicate fiber and alumina fiber in sequence and stir for 5 minutes;

[0072] S23, add expanded perlite, expanded vermiculite, floating beads, mica, hydroxypropyl cellulose, and sodium α-olefin sulfonate in sequence, and continue stirring for 4 minutes;

[0073] S24. Finally, add black silicate binder and white silicate binder and continue stirring for 10 minutes to obtain the fireproof and heat-insulating coating.

[0074] 3. Surface refractory layer powder

[0075] Table 1-3 Example 1 Refractory Layer Powder Ingredients

[0076] Serial number Raw material name Weight 1 diatomite 20 2 Closed-cell perlite (80 mesh) 12 3 Expanded Vermiculite (220 mesh) 80 4 Microbeads (180 mesh) 20 5 Alumina Fiber 200 6 Aluminum silicate fiber 500 7 Silicon carbide powder 10 8 Zirconium-containing aluminum silicate fiber 4 9 Polyvinyl alcohol powder 3 10 Latex powder 30 11 ultramarine 0.2

[0077] The preparation method of the facing refractory layer is as follows:

[0078] S31, weigh the raw materials in Table 1-3 according to the proportion;

[0079] S32, start the dry powder mixer, add the raw materials in sequence and stir for 30 minutes to obtain the facing refractory layer powder;

[0080] S33, spreading the facing refractory layer powder evenly on the aluminum foil cloth;

[0081] S34, prepare a water glass solution with a concentration of 10wt.%, spray the water glass solution on the flattened finishing refractory layer powder, and obtain the finishing refractory layer after drying.

[0082] 4. Construction of multi-layer fire protection system:

[0083] S1. Remove debris including rust, oil, dust, etc. from the surface of the steel structure;

[0084] S2. Apply a layer of epoxy zinc-rich anti-rust primer on the surface of the steel structure and then maintain it indoors for 24 hours;

[0085] S3, evenly apply the interface agent on the surface of the steel structure to form an interface layer;

[0086] S4. When the interface layer is not completely dry, prepare the coating according to the mass ratio of fireproof and heat-insulating coating to water of 100:180, spray or apply the coating on the surface of the interface layer to form a fireproof and heat-insulating coating layer; preferably, the first spraying is 3 to 5 mm, and each subsequent spraying or applying is 5 to 10 mm until the thickness reaches 30 mm;

[0087] S5. According to the area of ​​the steel structure, cut the facing coil of the facing refractory layer, evenly apply the interface agent on the bottom surface of the facing refractory layer, stick the facing refractory layer to the surface of the fire-retardant and heat-insulating coating layer and then gently press to fix it.

[0088] S6. Maintain the steel structure of S5 for 25 days.

[0089] Example 2

[0090] This embodiment discloses the multi-layer fire protection system and the construction method thereof of the present invention, which are specifically as follows:

[0091] 1. Interface agent:

[0092] Table 2-1 Ingredients of interface agent of Example 2

[0093]

[0094] The preparation method of the interface agent is as follows:

[0095] S11, weigh the raw materials in Table 2-1 according to the proportion;

[0096] S12, adding water into a blender, and pouring in 0.25 parts of alcohol ester twelve;

[0097] S13, start the mixer, set the mixer speed to 1500 r / min, slowly add hydroxypropyl cellulose ether, and stir for 20 min;

[0098] S14, adjust the mixer speed to 900r / min, and slowly add the solid mixed material into the mixing tank;

[0099] S15, pour in the flame retardant emulsion 907 while stirring;

[0100] S16, pour in the remaining alcohol ester 12;

[0101] S17. Reduce the speed of the mixer to 500 r / min, slowly add the vitrified microspheres, and continue stirring for 20 minutes to obtain a uniform and thick interface agent.

[0102] 2. Fireproof and heat-insulating coatings:

[0103] Table 2-2 Ingredients of fireproof and heat-insulating coating of Example 2

[0104]

[0105]

[0106] The preparation method of the fireproof and heat-insulating coating is as follows:

[0107] S21, weigh the raw materials in Table 2-2 according to the proportion;

[0108] S22, start the mixer, add zirconium-containing aluminum silicate fiber and alumina fiber in sequence and stir for 5 minutes;

[0109] S23, add expanded perlite, expanded vermiculite, floating beads, mica, hydroxypropyl cellulose, and sodium α-olefin sulfonate in sequence, and continue stirring for 4 minutes;

[0110] S24. Finally, add black silicate binder and white silicate binder and continue stirring for 10 minutes to obtain the fireproof and heat-insulating coating.

[0111] 3. Surface refractory layer powder

[0112] Table 2-3 Example 2 Refractory Layer Powder Ingredients

[0113] Serial number Raw material name Weight 1 diatomite 15 2 Closed-cell perlite (100 mesh) 8 3 Expanded Vermiculite (200 mesh) 60 4 Microbeads (150 mesh) 15 5 Alumina Fiber 150 6 Aluminum silicate fiber 300 7 Silicon carbide powder 8 8 Zirconium-containing aluminum silicate fiber 2 9 Polyvinyl alcohol powder 2 10 Latex powder 18 11 ultramarine 0.1

[0114] The preparation method of the facing refractory layer is as follows:

[0115] S31, weigh the raw materials in Table 2-3 according to the proportion;

[0116] S32, start the dry powder mixer, add the raw materials in sequence and stir for 30 minutes to obtain the facing refractory layer powder;

[0117] S33, spreading the facing refractory layer powder evenly on the aluminum foil cloth;

[0118] S34, prepare a water glass solution with a concentration of 20wt.%, spray the water glass solution on the flattened finishing refractory layer powder, and obtain the finishing refractory layer after drying.

[0119] 4. Construction of multi-layer fire protection system:

[0120] S1. Remove debris including rust, oil, dust, etc. from the surface of the steel structure;

[0121] S2. Apply a layer of epoxy zinc-rich anti-rust primer on the surface of the steel structure and then maintain it indoors for 24 hours;

[0122] S3, evenly apply the interface agent on the surface of the steel structure to form an interface layer;

[0123] S4. When the interface layer is not completely dry, prepare the coating according to the mass ratio of fireproof and heat-insulating coating to water of 100:200, spray or apply the coating on the surface of the interface layer to form a fireproof and heat-insulating coating layer; preferably, the first spraying is 3 to 5 mm, and each subsequent spraying or applying is 5 to 10 mm until the thickness reaches 30 mm;

[0124] S5. According to the area of ​​the steel structure, cut the facing coil of the facing refractory layer, evenly apply the interface agent on the bottom surface of the facing refractory layer, stick the facing refractory layer to the surface of the fire-retardant and heat-insulating coating layer and then gently press to fix it.

[0125] S6. Maintain the steel structure of S5 for 30 days.

[0126] Example 3

[0127] This embodiment discloses the multi-layer fire protection system and the construction method thereof of the present invention, which are specifically as follows:

[0128] 1. Interface agent:

[0129] Table 3-1 Ingredients of interface agent of Example 3

[0130]

[0131] The preparation method of the interface agent is as follows:

[0132] S11, weigh the raw materials in Table 3-1 according to the proportion;

[0133] S12, adding water to the dry powder mixer, and pouring in 0.75 parts of alcohol ester twelve;

[0134] S13, start the mixer, set the mixer speed to 1500 r / min, slowly add hydroxypropyl cellulose ether, and stir for 20 min;

[0135] S14, adjust the mixer speed to 900r / min, and slowly add the solid mixed material into the mixing tank;

[0136] S15, pour in the flame retardant emulsion 907 while stirring;

[0137] S16, pour in the remaining alcohol ester 12;

[0138] S17. Reduce the speed of the mixer to 500 r / min, slowly add the vitrified microspheres, and continue stirring for 20 minutes to obtain a uniform and thick interface agent.

[0139] 2. Fireproof and heat-insulating coatings:

[0140] Table 3-2 Ingredients of fireproof and heat-insulating coating of Example 3

[0141] Serial number Raw material name Weight 1 Black silicate binder 1000 2 White silicate binder 200 3 Expanded Perlite 180 4 Expanded Vermiculite 1000 5 Floating beads 30 6 Mica 300 7 Hydroxypropyl Cellulose 2 8 Sodium α-olefin sulfonate 0.3 9 Zirconium-containing aluminum silicate fiber 3 10 Alumina Fiber 60

[0142] The preparation method of the fireproof and heat-insulating coating is as follows:

[0143] S21, weigh the raw materials in Table 3-2 according to the proportion;

[0144] S22, start the mixer, add zirconium-containing aluminum silicate fiber and alumina fiber in sequence and stir for 5 minutes;

[0145] S23, add expanded perlite, expanded vermiculite, floating beads, mica, hydroxypropyl cellulose, and sodium α-olefin sulfonate in sequence, and continue stirring for 4 minutes;

[0146] S24. Finally, add black silicate binder and white silicate binder and continue stirring for 10 minutes to obtain the fireproof and heat-insulating coating.

[0147] 3. Surface refractory layer powder

[0148] Table 3-3 Example 3 Refractory Layer Powder Ingredients

[0149]

[0150]

[0151] The preparation method of the facing refractory layer is as follows:

[0152] S31, weigh the raw materials in Table 3-3 according to the proportion;

[0153] S32, start the dry powder mixer, add the raw materials in sequence and stir for 30 minutes to obtain the facing refractory layer powder;

[0154] S33, spreading the facing refractory layer powder evenly on the aluminum foil cloth;

[0155] S34, preparing a water glass solution with a concentration of 5wt.%, spraying the water glass solution on the flattened finishing refractory layer powder, and obtaining the finishing refractory layer after drying.

[0156] 4. Construction of multi-layer fire protection system:

[0157] S1. Remove debris including rust, oil, dust, etc. from the surface of the steel structure;

[0158] S2. Apply a layer of epoxy zinc-rich anti-rust primer on the surface of the steel structure and then maintain it indoors for 24 hours;

[0159] S3, evenly apply the interface agent on the surface of the steel structure to form an interface layer;

[0160] S4. When the interface layer is not completely dry, prepare the coating according to the mass ratio of fireproof and heat-insulating coating to water of 100:220, spray or apply the coating on the surface of the interface layer to form a fireproof and heat-insulating coating layer; preferably, the first spraying is 3 to 5 mm, and each subsequent spraying or applying is 5 to 10 mm until the thickness reaches 30 mm;

[0161] S5. According to the area of ​​the steel structure, cut the facing coil of the facing fire-resistant layer, evenly apply the interface agent on the surface of the fire-retardant and heat-insulating coating layer, stick the facing fire-resistant layer to the surface of the fire-retardant and heat-insulating coating layer and then gently press to fix it.

[0162] S6. Maintain the steel structure of S5 for 25 days.

[0163] Example 4

[0164] This embodiment discloses the multi-layer fire protection system and the construction method thereof of the present invention, which are specifically as follows:

[0165] 1. Interface agent:

[0166] Table 4-1 Ingredients of interface agent of Example 4

[0167]

[0168]

[0169] The preparation method of the interface agent is as follows:

[0170] S11, weigh the raw materials in Table 4-1 according to the proportion;

[0171] S12, adding water into a blender, and pouring in 0.625 parts of alcohol ester twelve;

[0172] S13, start the mixer, set the mixer speed to 1500 r / min, slowly add hydroxypropyl cellulose ether, and stir for 20 min;

[0173] S14, adjust the mixer speed to 900r / min, and slowly add the solid mixed material into the mixing tank;

[0174] S15, pouring in the flame retardant emulsion 907 while stirring;

[0175] S16, pour in the remaining alcohol ester 12;

[0176] S17. Reduce the speed of the mixer to 500 r / min, slowly add the vitrified microspheres, and continue stirring for 20 minutes to obtain a uniform and thick interface agent.

[0177] 2. Fireproof and heat-insulating coatings:

[0178] Table 4-2 Ingredients of fireproof and heat-insulating coating of Example 4

[0179] Serial number Raw material name Weight 1 Black silicate binder 1100 2 White silicate binder 220 3 Expanded Perlite 140 4 Expanded Vermiculite 800 5 Floating beads 15 6 Mica 180 7 Hydroxypropyl Cellulose 4 8 Sodium α-olefin sulfonate 0.25 9 Zirconium-containing aluminum silicate fiber 2.3 10 Alumina Fiber 40

[0180] The preparation method of the fireproof and heat-insulating coating is as follows:

[0181] S21, weigh the raw materials in Table 4-2 according to the proportion;

[0182] S22, start the mixer, add zirconium-containing aluminum silicate fiber and alumina fiber in sequence and stir for 5 minutes;

[0183] S23, add expanded perlite, expanded vermiculite, floating beads, mica, hydroxypropyl cellulose, and sodium α-olefin sulfonate in sequence, and continue stirring for 4 minutes;

[0184] S24. Finally, add black silicate binder and white silicate binder and continue stirring for 10 minutes to obtain the fireproof and heat-insulating coating.

[0185] 3. Surface refractory layer powder

[0186] Table 4-3 Example 4 Refractory Layer Powder Ingredients

[0187] Serial number Raw material name Weight 1 diatomite 25 2 Closed-cell perlite (90 mesh) 10 3 Expanded Vermiculite (175 mesh) 90 4 Microbeads (120 mesh) 22 5 Alumina Fiber 175 6 Aluminum silicate fiber 610 7 Silicon carbide powder 15 8 Zirconium-containing aluminum silicate fiber 4 9 Polyvinyl alcohol powder 3 10 Latex powder 30 11 ultramarine 0.2

[0188] The preparation method of the facing refractory layer is as follows:

[0189] S31, weigh the raw materials in Table 4-3 according to the proportion;

[0190] S32, start the dry powder mixer, add the raw materials in sequence and stir for 30 minutes to obtain the facing refractory layer powder;

[0191] S33, spreading the facing refractory layer powder evenly on the aluminum foil cloth;

[0192] S34, prepare a water glass solution with a concentration of 10%, spray the water glass solution on the flattened finishing refractory layer powder, and obtain the finishing refractory layer after drying.

[0193] 4. Construction of multi-layer fire protection system:

[0194] S1. Remove debris including rust, oil, dust, etc. from the surface of the steel structure;

[0195] S2. Apply a layer of epoxy zinc-rich anti-rust primer on the surface of the steel structure and then maintain it indoors for 24 hours;

[0196] S3, evenly apply the interface agent on the surface of the steel structure to form an interface layer;

[0197] S4. When the interface layer is not completely dry, prepare the coating according to the mass ratio of fireproof and heat-insulating coating to water of 100:180, spray or apply the coating on the surface of the interface layer to form a fireproof and heat-insulating coating layer; preferably, the first spraying is 3 to 5 mm, and each subsequent spraying or applying is 5 to 10 mm until the thickness reaches 30 mm;

[0198] S5. According to the area of ​​the steel structure, cut the facing coil of the facing fire-resistant layer, evenly apply the interface agent on the bottom surface of the facing fire-resistant layer or the surface of the fire-retardant and heat-insulating coating layer, stick the facing fire-resistant layer to the surface of the fire-retardant and heat-insulating coating layer and then gently press to fix it.

[0199] S6. Maintain the steel structure of S5 for 28 days.

[0200] Example 5

[0201] This embodiment discloses the multi-layer fire protection system and the construction method thereof of the present invention, which are specifically as follows:

[0202] 1. Interface agent:

[0203] Table 5-1 Ingredients of interface agent in Example 5

[0204]

[0205] The preparation method of the interface agent is as follows:

[0206] S11, weigh the raw materials in Table 5-1 according to the proportion;

[0207] S12, adding water to the blender, and pouring in 0.375 parts of alcohol ester twelve;

[0208] S13, start the mixer, set the mixer speed to 1500 r / min, slowly add hydroxypropyl cellulose ether, and stir for 20 min;

[0209] S14, adjust the mixer speed to 900r / min, and slowly add the solid mixed material into the mixing tank;

[0210] S15, pouring in the flame retardant emulsion 907 while stirring;

[0211] S16, pour in the remaining alcohol ester 12;

[0212] S17. Reduce the speed of the mixer to 500 r / min, slowly add the vitrified microspheres, and continue stirring for 20 minutes to obtain a uniform and thick interface agent.

[0213] 2. Fireproof and heat-insulating coatings:

[0214] Table 5-2 Ingredients of fireproof and heat-insulating coating of Example 5

[0215]

[0216]

[0217] The preparation method of the fireproof and heat-insulating coating is as follows:

[0218] S21, weigh the raw materials in Table 5-2 according to the proportion;

[0219] S22, start the mixer, add zirconium-containing aluminum silicate fiber and alumina fiber in sequence and stir for 5 minutes;

[0220] S23, add expanded perlite, expanded vermiculite, floating beads, mica, hydroxypropyl cellulose, and sodium α-olefin sulfonate in sequence, and continue stirring for 4 minutes;

[0221] S24. Finally, add black silicate binder and white silicate binder and continue stirring for 10 minutes to obtain the fireproof and heat-insulating coating.

[0222] 3. Surface refractory layer powder

[0223] Table 5-3 Example 5 Refractory Layer Powder Ingredients

[0224] Serial number Raw material name Weight 1 diatomite 18 2 Closed-cell perlite (110 mesh) 14 3 Expanded Vermiculite (210 mesh) 100 4 Microbeads (165 mesh) 25 5 Alumina Fiber 210 6 Aluminum silicate fiber 680 7 Silicon carbide powder 13 8 Zirconium-containing aluminum silicate fiber 6 9 Polyvinyl alcohol powder 8 10 Latex powder 35 11 ultramarine 0.21

[0225] The preparation method of the facing refractory layer is as follows:

[0226] S31, weigh the raw materials in Table 5-3 according to the proportion;

[0227] S32, start the dry powder mixer, add the raw materials in sequence and stir for 30 minutes to obtain the facing refractory layer powder;

[0228] S33, spreading the facing refractory layer powder evenly on the aluminum foil cloth;

[0229] S34, prepare a water glass solution with a concentration of 10%, spray the water glass solution on the flattened finishing refractory layer powder, and obtain the finishing refractory layer after drying.

[0230] 4. Construction of multi-layer fire protection system:

[0231] S1. Remove debris including rust, oil, dust, etc. from the surface of the steel structure;

[0232] S2. Apply a layer of epoxy zinc-rich anti-rust primer on the surface of the steel structure and then maintain it indoors for 24 hours;

[0233] S3, evenly apply the interface agent on the surface of the steel structure to form an interface layer;

[0234] S4. When the interface layer is not completely dry, prepare the coating according to the mass ratio of fireproof and heat-insulating coating to water of 100:250, spray or apply the coating on the surface of the interface layer to form a fireproof and heat-insulating coating layer; preferably, the first spraying is 3 to 5 mm, and each subsequent spraying or applying is 5 to 10 mm until the thickness reaches 30 mm;

[0235] S5. According to the area of ​​the steel structure, cut the facing coil of the facing fire-resistant layer, evenly apply the interface agent on the surface of the fire-retardant and heat-insulating coating layer, stick the facing fire-resistant layer to the surface of the fire-retardant and heat-insulating coating layer and then gently press to fix it.

[0236] S6. Maintain the steel structure of S5 for 28 days.

[0237] Example 6

[0238] This embodiment discloses the multi-layer fire protection system and the construction method thereof of the present invention, which are specifically as follows:

[0239] 1. Interface agent:

[0240] Table 6-1 Ingredients of interface agent of Example 6

[0241]

[0242] The preparation method of the interface agent is as follows:

[0243] S11, weigh the raw materials in Table 6-1 according to the proportion;

[0244] S12, adding water into a blender, and pouring in 0.45 parts of alcohol ester twelve;

[0245] S13, start the mixer, set the mixer speed to 1500 r / min, slowly add hydroxypropyl cellulose ether, and stir for 20 min;

[0246] S14, adjust the mixer speed to 900r / min, and slowly add the solid mixed material into the mixing tank;

[0247] S15, pouring in the flame retardant emulsion 907 while stirring;

[0248] S16, pour in the remaining alcohol ester 12;

[0249] S17. Reduce the speed of the mixer to 500 r / min, slowly add the vitrified microspheres, and continue stirring for 20 minutes to obtain a uniform and thick interface agent.

[0250] 2. Fireproof and heat-insulating coatings:

[0251] Table 6-2 Ingredients of fireproof and heat-insulating coating of Example 6

[0252] Serial number Raw material name Weight 1 Black silicate binder 1050 2 White silicate binder 168 3 Expanded Perlite 135 4 Expanded Vermiculite 930 5 Floating beads 25 6 Mica 250 7 Hydroxypropyl Cellulose 2.5 8 Sodium α-olefin sulfonate 0.18 9 Zirconium-containing aluminum silicate fiber 4.6 10 Alumina Fiber 50

[0253] The preparation method of the fireproof and heat-insulating coating is as follows:

[0254] S21, weigh the raw materials in Table 6-2 according to the proportion;

[0255] S22, start the mixer, add zirconium-containing aluminum silicate fiber and alumina fiber in sequence and stir for 5 minutes;

[0256] S23, add expanded perlite, expanded vermiculite, floating beads, mica, hydroxypropyl cellulose, and sodium α-olefin sulfonate in sequence, and continue stirring for 4 minutes;

[0257] S24. Finally, add black silicate binder and white silicate binder and continue stirring for 10 minutes to obtain the fireproof and heat-insulating coating.

[0258] 3. Surface refractory layer powder

[0259] Table 6-3 Example 6 Refractory Layer Powder Ingredients

[0260]

[0261]

[0262] The preparation method of the facing refractory layer is as follows:

[0263] S31, weigh the raw materials in Table 6-3 according to the proportion;

[0264] S32, start the dry powder mixer, add the raw materials in sequence and stir for 30 minutes to obtain the facing refractory layer powder;

[0265] S33, spreading the facing refractory layer powder evenly on the aluminum foil cloth;

[0266] S34, prepare a water glass solution with a concentration of 10%, spray the water glass solution on the flattened finishing refractory layer powder, and obtain the finishing refractory layer after drying.

[0267] 4. Construction of multi-layer fire protection system:

[0268] S1. Remove debris including rust, oil, dust, etc. from the surface of the steel structure;

[0269] S2. Apply a layer of epoxy zinc-rich anti-rust primer on the surface of the steel structure and then maintain it indoors for 24 hours;

[0270] S3, evenly apply the interface agent on the surface of the steel structure to form an interface layer;

[0271] S4. When the interface layer is not completely dry, prepare the coating according to the mass ratio of fireproof and heat-insulating coating to water of 100:210, spray or apply the coating on the surface of the interface layer to form a fireproof and heat-insulating coating layer; preferably, the first spraying is 3 to 5 mm, and each subsequent spraying or applying is 5 to 10 mm until the thickness reaches 30 mm;

[0272] S5. According to the area of ​​the steel structure, cut the facing coil of the facing fire-resistant layer, evenly apply the interface agent on the surface of the fire-retardant and heat-insulating coating layer, stick the facing fire-resistant layer to the surface of the fire-retardant and heat-insulating coating layer and then gently press to fix it.

[0273] S6. Maintain the steel structure of S5 for 30 days.

[0274] Test Example 1

[0275] This test example discloses the performance test of the multi-layer fire protection system of the present invention.

[0276] 1. Fire resistance test

[0277] During the fire resistance test, four standard cover plates are covered on the surface of the steel structure (specifically steel beams). The cover plates are made of 800kg / m 3 The lightweight concrete slab is 150mm thick, 1000mm long and 600mm wide. A layer of aluminum silicate fiber wool is set between the cover plate and the upper flange of the beam, and its width is equal to the width of the upper flange of the beam. The specimen is loaded with four-point concentrated loads (simulating uniformly distributed loads). A total of 12 thermocouples are arranged inside the steel beam. The calculated span of the steel beam is 4200mm, and the total external load is 207kN.

[0278] Physical and chemical performance test pieces were sampled according to the requirements of GB14907-2018 "Steel Structure Fire Retardant Coatings". The results are shown in the following table:

[0279] Table 7 Test results

[0280]

[0281] After the test, the steel beam is removed from the refractory furnace. The composite fire protection system of the present invention can meet the 4.0h fire resistance requirement; the dry density is 411 (kg / m 3 ), less than the standard requirement of 650 (kg / m 3 );Freeze-thaw cycle resistance, heat exposure resistance, and moisture and heat resistance also meet the standard requirements.

[0282] 2. Outdoor exposure dripping natural aging test

[0283] In order to investigate the outdoor natural aging effect of the multi-layer fire protection system of the present invention, an outdoor aging test was conducted.

[0284] (1) Take a 1400mm×1400mm×3mm steel plate;

[0285] (2) Apply a layer of epoxy zinc-rich anti-rust paint on one side of the steel plate, and then apply a layer of epoxy micaceous iron intermediate paint 2 hours later, and let it dry naturally for 24 hours;

[0286] (3) The multi-layer fire protection system of the present invention is applied to a steel plate with a total thickness of 40 mm;

[0287] (4) After 7 days of natural curing, move the steel plate coated with the multi-layer fire protection system to the eaves so that water from the eaves on rainy days can directly wash the multi-layer fire protection system;

[0288] (5) After one year, scrape off the coating and observe the coating damage effect.

[0289] The test results are as follows Figure 2 and Figure 3 shown.

[0290] from Figure 2 and Figure 3 It can be seen that:

[0291] (1) Due to long-term immersion in water, the bottom of the fire-retardant coating is relatively damp, and moss about 40 mm thick has grown, and the coating is intact where the moss grows;

[0292] (2) The scraped coating is relatively fresh and has no obvious damage;

[0293] (3) The fire-retardant coating has no abnormal phenomena such as hollowing and cracking.

[0294] In summary, the multi-layer fire protection system of the present invention can provide long-term fire protection for steel structures.

[0295] The composite fire protection system of the present invention is compared with the test report of the non-expansive steel structure fire retardant coating produced by the main representative manufacturers of fire retardant coatings in the prior art, and the results are as follows:

[0296] Table 8 Technical index analysis of multi-layer fire protection system

[0297]

[0298] The data for serial numbers 1 to 3 in Table 8 are from the website of the Fire Products Conformity Assessment Center of the Ministry of Emergency Management.

[0299] It can be seen from the above table that the composite fire protection system of the present invention exhibits excellent thermal insulation performance compared with the prior art, has a lower internal temperature of the steel beam at 4h, and has a lower deformation; at the end of the test, the composite fire protection system of the present invention is lower.

[0300] Finally, it should be noted that the above embodiments are only preferred embodiments of the present invention to illustrate the technical solutions of the present invention, rather than limiting them, and certainly not limiting the patent scope of the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. In other words, any changes or modifications made to the main design concept and spirit of the present invention that have no substantive significance, and the technical problems they solve are still consistent with the present invention, should be included in the protection scope of the present invention. In addition, the direct or indirect application of the technical solutions of the present invention in other related technical fields is also included in the patent protection scope of the present invention.

Claims

1. A multi-layer fire protection system, characterized in that: It includes an interface layer, a fireproof and heat-insulating layer and a finishing refractory layer; wherein, the interface layer is formed by evenly coating the interface agent on the surface of the steel structure; the fireproof and heat-insulating coating layer is formed by smearing the fireproof and heat-insulating coating on the surface of the interface layer; the finishing refractory layer is composed of a finishing coil coated with finishing refractory layer powder.

2. A multi-layer fire protection system according to claim 1, characterized in that: The interface agent is made of the following raw materials in parts by weight: 30-40 parts of flame retardant emulsion 907, 25-40 parts of solid mixture, 1-3 parts of alcohol ester dodecahydrate, 15-30 parts of glass microspheres, 0.08-0.15 parts of hydroxypropyl cellulose ether, and 10-40 parts of water; Preferably, the interface agent is made of the following raw materials in parts by weight: 90740 parts of flame retardant emulsion, 35 parts of solid mixture, 2 parts of alcohol ester, 22 parts of glass microspheres, 0.1 parts of hydroxypropyl cellulose ether, and 20-30 parts of water.

3. A multi-layer fire protection system according to claim 2, characterized in that: The solid mixture includes silicon micropowder, alumina, and bentonite in a mass ratio of 6-10:0.3-1.5:0.05-0.15; Preferably, the solid mixture includes silicon micropowder, alumina and bentonite in a mass ratio of 8:1:0.

1.

4. A multi-layer fire protection system according to claim 2 or 3, characterized in that: The preparation method of the interface agent is as follows: S11, weighing the raw materials in parts by weight; S12, adding water into a blender, and pouring in a portion of alcohol ester 12, preferably, the mass of the portion of alcohol ester 12 is 1 / 2 of the total weight of alcohol ester 12; S13, start the stirrer, slowly add hydroxypropyl cellulose ether and stir, preferably, the stirring speed is 1200-1800 r / min, and the stirring time is 15-30 min; S14, reducing the stirring speed, slowly adding the solid mixture for stirring, preferably, the stirring speed is 800-1000 r / min, and the stirring time is 15-25 min; S15, adding emulsion flame retardant emulsion 907 while stirring; S16, pour in the remaining alcohol ester 12; S17, reducing the stirring speed, slowly adding the vitrified microbeads and stirring to obtain the interface agent. Preferably, the stirring speed is 450-600 r / min, and the stirring time is 15-25 min.

5. A multi-layer fire protection system according to claim 1, characterized in that: The fireproof and heat-insulating coating comprises the following raw materials in parts by weight: 800-1200 parts of black silicate binder, 150-220 parts of white silicate binder, 120-180 parts of expanded perlite, 650-1000 parts of expanded vermiculite, 10-30 parts of floating beads, 150-300 parts of mica, 1.0-5 parts of hydroxypropyl cellulose ether, 0.15-0.3 parts of sodium α-olefin sulfonate, 2-5 parts of zirconium-containing aluminum silicate fiber, and 35-60 parts of alumina fiber; Preferably, the fireproof and heat-insulating coating is made of the following raw materials in parts by weight: 900 parts of black silicate binder, 180 parts of white silicate binder, 150 parts of expanded perlite, 850 parts of expanded vermiculite, 20 parts of floating beads, 220 parts of mica, 3 parts of hydroxypropyl cellulose, 0.2 parts of sodium α-olefin sulfonate, 4 parts of zirconium-containing aluminum silicate fiber, and 50 parts of alumina fiber.

6. A multi-layer fire protection system according to claim 5, characterized in that: The preparation method of the fireproof and heat-insulating coating is as follows: S21, weighing the raw materials in parts by weight; S22, start the mixer, add zirconium-containing aluminum silicate fiber and aluminum oxide fiber in sequence and stir, preferably, the stirring time is 5 to 10 minutes; S23, add expanded perlite, expanded vermiculite, floating beads, mica, hydroxypropyl cellulose, and sodium α-olefin sulfonate in sequence and continue stirring. Preferably, the stirring time is 3 to 5 minutes; S24. Finally, add the black silicate binder and the white silicate binder and continue stirring to obtain the fireproof and heat-insulating coating. Preferably, the stirring time is 5 to 10 minutes.

7. A multi-layer fire protection system according to claim 1, characterized in that: The facing refractory layer powder is made of the following raw materials in parts by weight: 15-30 parts of diatomaceous earth, 8-15 parts of closed-cell perlite, 60-100 parts of expanded vermiculite, 15-25 parts of microspheres, 150-280 parts of alumina fiber, 300-700 parts of aluminum silicate fiber, 8-15 parts of silicon carbide powder, 2-6 parts of zirconium-containing aluminum silicate fiber, 2-8 parts of polyvinyl alcohol powder, 18-40 parts of latex powder, and 0.1-0.3 parts of ultramarine. Preferably, the facing refractory layer powder is made of the following raw materials in parts by weight: 20 parts of diatomaceous earth, 12 parts of closed-cell perlite, 80 parts of expanded vermiculite, 20 parts of microspheres, 200 parts of alumina fiber, 500 parts of aluminum silicate fiber, 10 parts of silicon carbide powder, 4 parts of zirconium-containing aluminum silicate fiber, 3 parts of polyvinyl alcohol powder, 30 parts of latex powder, and 0.2 parts of ultramarine.

8. A multi-layer fire protection system according to claim 7, characterized in that: The particle size of the closed-cell perlite is 8 to 120 meshes, preferably 20 meshes; Or / and the particle size of expanded vermiculite is 15 to 100 meshes, preferably 40 meshes; The particle size of the microbeads is 10 to 180 mesh, preferably 50 mesh.

9. A multi-layer fire protection system according to claim 7, characterized in that: The preparation method of the facing refractory layer is as follows: S31, weighing the raw materials in parts by weight; S32, start the mixer, add the raw materials in sequence and stir to obtain a facing refractory layer powder, preferably, the stirring time is 20 to 40 minutes; S33, evenly spreading the facing refractory layer powder on the facing coiled material; S34, preparing a binder solution, spraying the binder solution on the flattened facing refractory layer powder, and obtaining the facing refractory layer after drying; preferably, the thickness of the facing refractory layer is 0.2 to 2 mm; Preferably, the binder solution is a water glass solution, more preferably a water glass solution with a mass concentration of 5 to 20%, and further preferably a water glass solution with a mass concentration of 10%.

10. A construction method for a multi-layer fire protection system according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. Remove debris from the surface of the steel structure, including rust, oil stains, and dust; S2. Apply a layer of anti-rust primer on the surface of the steel structure and maintain it; preferably, the anti-rust primer is an epoxy zinc-rich anti-rust primer, and the coating thickness of the anti-rust primer is 40 to 80 μm; preferably, the anti-rust primer is maintained indoors; further preferably, the anti-rust primer is maintained indoors for 8 to 60 hours, more preferably for 24 hours; S3, evenly apply the interface agent on the surface of the steel structure to form an interface layer; S4. When the interface layer is not completely dry, prepare the coating according to the mass ratio of fireproof and heat-insulating coating to water of 100:(180-250), spray or apply the coating on the surface of the interface layer to form a fireproof and heat-insulating coating layer; preferably, the first spraying is 3-5 mm, and each subsequent spraying or applying is 10-20 mm, until the thickness reaches 36-39 mm; S5. According to the area of ​​the steel structure, cut the facing coil of the facing fire-resistant layer, evenly apply the interface agent on the bottom surface of the facing fire-resistant layer or the surface of the fire-retardant and heat-insulating coating layer, stick the facing fire-resistant layer to the surface of the fire-retardant and heat-insulating coating layer and then gently press to fix it. S6. Curing the steel structure completed in S5, preferably, curing for 25 to 30 days.